Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683 | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | O | EN 573-3, EN 546 | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | O | EN 573-3, EN 546 | A50 | |||
4.0 % Show Material materials with Dehnung of 4.0 % | O | EN 573-3, EN 546 | A50 | |||
7.0 % Show Material materials with Dehnung of 7.0 % | O | EN 573-3, EN 546 | A50 | |||
12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3, EN 546, EN 683 | A50 | |||
16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3, EN 546, EN 683 | A50 | |||
19.0 % Show Material materials with Dehnung of 19.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3, EN 683 | A50 | |||
21.0 % Show Material materials with Dehnung of 21.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
24.0 % Show Material materials with Dehnung of 24.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
25.0 % Show Material materials with Dehnung of 25.0 % | O | EN 573-3, EN 485 | A50 | |||
30.0 % Show Material materials with Dehnung of 30.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 30.0 % Show Material materials with Dehnung of 30.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 35.0 % Show Material materials with Dehnung of 35.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683 | |||
Härte, Brinell | 25.0 [-] Show Material materials with Härte, Brinell of 25.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 25.0 [-] Show Material materials with Härte, Brinell of 25.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 8000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 8000 Series Aluminium | ||||
Zugfestigkeit | 50.0 - 110.0 MPa Show Material materials with Zugfestigkeit of 50.0 - 110.0 MPa | O | EN 573-3, EN 546 | |||
55.0 - 115.0 MPa Show Material materials with Zugfestigkeit of 55.0 - 115.0 MPa | O | EN 573-3, EN 546 | ||||
55.0 - 120.0 MPa Show Material materials with Zugfestigkeit of 55.0 - 120.0 MPa | O | EN 573-3, EN 546 | ||||
65.0 - 130.0 MPa Show Material materials with Zugfestigkeit of 65.0 - 130.0 MPa | O | EN 573-3, EN 546, EN 683 | ||||
80.0 - 120.0 MPa Show Material materials with Zugfestigkeit of 80.0 - 120.0 MPa | O | EN 573-3, EN 1396 | ||||
85.0 MPa Show Material materials with Zugfestigkeit of 85.0 MPa | O | EN 573-3, EN 485 | ||||
20.0 °C | 75.0 - 110.0 MPa Show Material materials with Zugfestigkeit of 75.0 - 110.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 75.0 - 115.0 MPa Show Material materials with Zugfestigkeit of 75.0 - 115.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 80.0 - 110.0 MPa Show Material materials with Zugfestigkeit of 80.0 - 110.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 80.0 - 115.0 MPa Show Material materials with Zugfestigkeit of 80.0 - 115.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683 | ||
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683 | |||
Schmelzpunkt | 640.0 - 655.0 °C Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683 | |||
Spezifische Wärmekapazität | 920.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 920.0 J/(kg·K) | Typical for Wrought 8000 Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 220.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 34000000.0 - 35000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34000000.0 - 35000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683 | Flat |
spezifischer Widerstand | 2.86e-08 - 2.94e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.86e-08 - 2.94e-08 Ω·m | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683 | |
Eisen | 0.5 - 1.0 % Show Material materials with Eisen of 0.5 - 1.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683 | Flat |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683 | Flat |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683 | |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683 | Flat |
Silizium | 0.4 - 0.8 % Show Material materials with Silizium of 0.4 - 0.8 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683 | Flat |
Titan | 0.05 Show Material materials with Titan of 0.05 | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683 | Flat |