Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | ||
20.0 °C | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Flat, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 75.0 MPa Show Material materials with Bending Fatigue Strength of 75.0 MPa | H18 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | |||
Biegewinkel 90° | 1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H18 | EN 573-3, EN 485 | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H18 | EN 573-3, EN 485 | ||||
3.0 °/t Show Material materials with Biegewinkel 90° of 3.0 °/t | H18 | EN 573-3, EN 485 | ||||
Dehnung | -196.0 °C | 30.0 % Show Material materials with Dehnung of 30.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | ||
-80.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
-20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
1.0 % Show Material materials with Dehnung of 1.0 % | H18 | EN 573-3, EN 485, EN 546, EN 683 | A50 | |||
2.0 % Show Material materials with Dehnung of 2.0 % | H18 | EN 573-3, EN 1592 | A100 | |||
2.0 % Show Material materials with Dehnung of 2.0 % | H18 | EN 573-3, EN 485, EN 754 | A50 | |||
3.0 % Show Material materials with Dehnung of 3.0 % | H18 | EN 573-3, EN 1301 | ||||
3.0 % Show Material materials with Dehnung of 3.0 % | H18 | EN 573-3, EN 754 | A100 | |||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Wire | A100 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Flat, Wire | A10 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
100.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
150.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
200.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
260.0 °C | 60.0 % Show Material materials with Dehnung of 60.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
320.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
370.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
Elastizitätsmodul | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 65.0 GPa | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Flat, Wire | ||
Härte, Brinell | 58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H18 | EN 573-3, EN 485 | |||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Wire | ||
20.0 °C | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | |||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Schubmodule of 24.0 - 26.5 GPa | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Flat, Wire | ||
Zugfestigkeit | -196.0 °C | 298.0 MPa Show Material materials with Zugfestigkeit of 298.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | ||
-80.0 °C | 225.0 MPa Show Material materials with Zugfestigkeit of 225.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | |||
-20.0 °C | 214.0 MPa Show Material materials with Zugfestigkeit of 214.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | |||
170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | H18 | EN 573-3, EN 1301 | ||||
180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | H18 | EN 573-3, EN 754 | ||||
185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | H18 | EN 573-3, EN 485, EN 683 | ||||
185.0 - 230.0 MPa Show Material materials with Zugfestigkeit of 185.0 - 230.0 MPa | H18 | EN 573-3, EN 546 | ||||
190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | H18 | EN 573-3, EN 1592 | ||||
20.0 °C | 100.0 MPa Show Material materials with Zugfestigkeit of 100.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513 | Tube | ||
20.0 °C | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | Wire | ||
20.0 °C | 165.0 - 205.0 MPa Show Material materials with Zugfestigkeit of 165.0 - 205.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 204.0 MPa Show Material materials with Zugfestigkeit of 204.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | |||
100.0 °C | 183.0 MPa Show Material materials with Zugfestigkeit of 183.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | |||
150.0 °C | 163.0 MPa Show Material materials with Zugfestigkeit of 163.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | |||
200.0 °C | 98.0 MPa Show Material materials with Zugfestigkeit of 98.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | |||
260.0 °C | 53.0 MPa Show Material materials with Zugfestigkeit of 53.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | |||
320.0 °C | 28.0 MPa Show Material materials with Zugfestigkeit of 28.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | |||
370.0 °C | 21.0 MPa Show Material materials with Zugfestigkeit of 21.0 MPa | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | ||
Schmelzpunkt | 645.0 - 655.0 °C Show Material materials with Schmelzpunkt of 645.0 - 655.0 °C | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | ||
Spezifische Wärmekapazität | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Flat, Wire | |
Wärmeleitfähigkeit | 20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 200.0 W/(m·K) | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Flat, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 22000000.0 - 28000000.0 S/m | H18 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Flat, Wire |
spezifischer Widerstand | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.57e-08 - 4.55e-08 Ω·m | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Tube, Flat, Wire |
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | Tube, Flat, Wire |
0.70 % Show Material materials with Eisen of 0.70 % | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Tube, Flat, Wire |
Magnesium | 0.3 % Show Material materials with Magnesium of 0.3 % | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Tube, Flat, Wire |
Mangan | 0.9 - 1.5 % Show Material materials with Mangan of 0.9 - 1.5 % | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Tube, Flat, Wire |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Tube, Flat, Wire |
Titan | 0.1 Show Material materials with Titan of 0.1 | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4 | Tube, Flat, Wire |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H18 | DIN 1725-1, VdTÜV WB 420-4, VdTÜV WB 513, EN 573-3, EN 573-4, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Tube, Flat, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |