DIN 1725-1 Grade 3.0525 H16

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMn1Mg0,5 is similarly to AlMn1 in its properties. It reaches strength up to F 25. The alloy belongs to the nature-hard aluminum materials. A strength increase can only occure by cold forming. It is very well hot and cold formable and is suitable to the deep-drawing (no lappet formation). The alloy AlMn1Mg0,5 is very well corrosion resistant and is sea water steady. As semi-finished material it is present in accordance with DIN 1788 and DIN 1745 only as sheet metal or strip. Application: Mainly in the packing for cans (lower parts), for menu bowls, for covers. In the building industry for claddings, roofings, for sun protection facilities (roller schutter, lamella net curtain) and for roll gates as well as for flexible pipes and in the construction of vehicles.

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM,AluKey zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValueConditionRelated StandardsShape

Dichte

2.72 g/cm³

Show Material materials with Dichte of 2.72 g/cm³

H16

EN 573-3, EN 1592, EN 485

20.0 °C

2.72 g/cm³

Show Material materials with Dichte of 2.72 g/cm³

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Mechanisch

PropertyTemperatureValueConditionRelated StandardsShapeComment

Biegewinkel 90°

1.0 °/t

Show Material materials with Biegewinkel 90° of 1.0 °/t

H16

EN 573-3, EN 485

1.5 °/t

Show Material materials with Biegewinkel 90° of 1.5 °/t

H16

EN 573-3, EN 485

2.5 °/t

Show Material materials with Biegewinkel 90° of 2.5 °/t

H16

EN 573-3, EN 485

Dehnung

1.0 %

Show Material materials with Dehnung of 1.0 %

H16

EN 573-3, EN 485

A50

2.0 %

Show Material materials with Dehnung of 2.0 %

H16

EN 573-3, EN 485

A50

5.0 %

Show Material materials with Dehnung of 5.0 %

H16

EN 573-3, EN 1592

A100

20.0 °C

2.0 %

Show Material materials with Dehnung of 2.0 %

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

A10

20.0 °C

3.0 %

Show Material materials with Dehnung of 3.0 %

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Elastizitätsmodul

70.0 GPa

Show Material materials with Elastizitätsmodul of 70.0 GPa

H16

EN 573-3, EN 1592, EN 485

20.0 °C

65.0 GPa

Show Material materials with Elastizitätsmodul of 65.0 GPa

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Härte, Brinell

61.0 [-]

Show Material materials with Härte, Brinell of 61.0 [-]

H16

EN 573-3, EN 485

20.0 °C

65.0 [-]

Show Material materials with Härte, Brinell of 65.0 [-]

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poissonzahl

0.33 [-]

Show Material materials with Poissonzahl of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Schubmodule

20.0 °C

26.5

Show Material materials with Schubmodule of 26.5

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Zugfestigkeit

195.0 - 240.0 MPa

Show Material materials with Zugfestigkeit of 195.0 - 240.0 MPa

H16

EN 573-3, EN 485

210.0 MPa

Show Material materials with Zugfestigkeit of 210.0 MPa

H16

EN 573-3, EN 1592

20.0 °C

195.0 - 235.0 MPa

Show Material materials with Zugfestigkeit of 195.0 - 235.0 MPa

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Thermisch

PropertyTemperatureValueConditionRelated StandardsShape

Koeffizient der thermischen Ausdehnung

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K

H16

EN 573-3, EN 1592, EN 485

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K

H16

EN 573-3, EN 1592, EN 485

Schmelzpunkt

630.0 - 654.0 °C

Show Material materials with Schmelzpunkt of 630.0 - 654.0 °C

H16

EN 573-3, EN 1592, EN 485

Spezifische Wärmekapazität

20.0 °C

893.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K)

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Wärmeleitfähigkeit

160.0 - 190.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 160.0 - 190.0 W/(m·K)

H16

EN 573-3, EN 1592, EN 485

20.0 °C

200.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 200.0 W/(m·K)

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Elektrisch

PropertyTemperatureValueConditionRelated StandardsShape

Elektrische Leitfähigkeit

23000000.0 - 25000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 25000000.0 S/m

H16

EN 573-3, EN 1592, EN 485

20.0 °C

28000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 28000000.0 S/m

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

spezifischer Widerstand

4e-08 - 4.35e-08 Ω·m

Show Material materials with spezifischer Widerstand of 4e-08 - 4.35e-08 Ω·m

H16

EN 573-3, EN 1592, EN 485

Chemical properties

PropertyValueConditionRelated StandardsShape

Chrom

0.1 %

Show Material materials with Chrom of 0.1 %

H16

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Sheet, Strip

Eisen

0.7 %

Show Material materials with Eisen of 0.7 %

H16

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

0.70 %

Show Material materials with Eisen of 0.70 %

H16

EN 573-3, EN 1592, EN 485

Kupfer

0.3 %

Show Material materials with Kupfer of 0.3 %

H16

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Sheet, Strip

Magnesium

0.2 - 0.6 %

Show Material materials with Magnesium of 0.2 - 0.6 %

H16

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Sheet, Strip

Mangan

1.0 - 1.5 %

Show Material materials with Mangan of 1.0 - 1.5 %

H16

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Sheet, Strip

Silizium

0.6 %

Show Material materials with Silizium of 0.6 %

H16

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Sheet, Strip

Titan

0.1 %

Show Material materials with Titan of 0.1 %

H16

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Sheet, Strip

Zink

0.25 %

Show Material materials with Zink of 0.25 %

H16

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Sheet, Strip

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Corrosion properties

Seawater: very good, weathering: very good

Workability