Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | O | EN 573-3, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | ||
20.0 °C | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 110.0 MPa Show Material materials with Bending Fatigue Strength of 110.0 MPa | O | EN 573-3, EN 1301, EN 1396, EN 1592, EN 485, EN 754, EN 755 | |||
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | O | EN 573-3, EN 14286, EN 485 | ||||
2.0 °/t Show Material materials with Biegewinkel 180° of 2.0 °/t | O | EN 573-3, EN 14286 | ||||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | O | EN 573-3, EN 485 | ||||
Dehnung | -196.0 °C | 42.2 % Show Material materials with Dehnung of 42.2 % | O | DIN 1725-1, EN 573-3, EN 573-4 | ||
-150.0 °C | 35.8 % Show Material materials with Dehnung of 35.8 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
-100.0 °C | 29.8 % Show Material materials with Dehnung of 29.8 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
-50.0 °C | 24.5 % Show Material materials with Dehnung of 24.5 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
14.0 % Show Material materials with Dehnung of 14.0 % | O | EN 573-3, EN 1396, EN 485, EN 754 | A50 | |||
15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3, EN 755 | A50 | |||
16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3, EN 1301 | ||||
16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3, EN 754 | A100 | |||
16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
17.0 % Show Material materials with Dehnung of 17.0 % | O | EN 573-3, EN 1592, EN 485, EN 755 | A100 | |||
18.0 % Show Material materials with Dehnung of 18.0 % | O | EN 573-3, EN 485 | A50 | |||
21.0 % Show Material materials with Dehnung of 21.0 % | O | EN 573-3, EN 14286 | A100 | |||
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A10 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod | A10 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Tube | A10 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Strip, Sheet | ||
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 21.1 % Show Material materials with Dehnung of 21.1 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
20.0 °C | 21.1 - 24.0 % Show Material materials with Dehnung of 21.1 - 24.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
20.0 °C | 24.0 % Show Material materials with Dehnung of 24.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
60.0 °C | 24.0 % Show Material materials with Dehnung of 24.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
100.0 °C | 24.0 % Show Material materials with Dehnung of 24.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
140.0 °C | 29.0 % Show Material materials with Dehnung of 29.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
180.0 °C | 50.0 % Show Material materials with Dehnung of 50.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
240.0 °C | 52.0 % Show Material materials with Dehnung of 52.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
300.0 °C | 62.0 % Show Material materials with Dehnung of 62.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
360.0 °C | 88.0 % Show Material materials with Dehnung of 88.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
Elastizitätsmodul | 70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | O | EN 573-3, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
20.0 °C | 68.0 - 72.0 GPa Show Material materials with Elastizitätsmodul of 68.0 - 72.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Härte, Brinell | 52.0 [-] Show Material materials with Härte, Brinell of 52.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 40.0 [-] Show Material materials with Härte, Brinell of 40.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Wire | ||
20.0 °C | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Strip, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Scherfestigkeit | 20.0 °C | 115.0 MPa Show Material materials with Scherfestigkeit of 115.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
Schubmodule | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | O | EN 573-3, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
20.0 °C | 27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Zugfestigkeit | -196.0 °C | 350.0 MPa Show Material materials with Zugfestigkeit of 350.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | ||
-150.0 °C | 275.0 MPa Show Material materials with Zugfestigkeit of 275.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
-100.0 °C | 240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
-50.0 °C | 227.0 MPa Show Material materials with Zugfestigkeit of 227.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
180.0 - 250.0 MPa Show Material materials with Zugfestigkeit of 180.0 - 250.0 MPa | O | EN 573-3, EN 754, EN 755 | ||||
190.0 - 240.0 MPa Show Material materials with Zugfestigkeit of 190.0 - 240.0 MPa | O | EN 573-3, EN 1396, EN 14286, EN 485 | ||||
190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | O | EN 573-3, EN 1592 | ||||
250.0 MPa Show Material materials with Zugfestigkeit of 250.0 MPa | O | EN 573-3, EN 1301 | ||||
20.0 °C | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube, Wire | ||
20.0 °C | 190.0 - 230.0 MPa Show Material materials with Zugfestigkeit of 190.0 - 230.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Strip, Sheet, Flat | ||
20.0 °C | 215.0 - 221.0 MPa Show Material materials with Zugfestigkeit of 215.0 - 221.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
20.0 °C | 215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
20.0 °C | 221.0 MPa Show Material materials with Zugfestigkeit of 221.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
100.0 °C | 212.0 MPa Show Material materials with Zugfestigkeit of 212.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
140.0 °C | 197.0 MPa Show Material materials with Zugfestigkeit of 197.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
180.0 °C | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
240.0 °C | 120.0 MPa Show Material materials with Zugfestigkeit of 120.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
300.0 °C | 85.0 MPa Show Material materials with Zugfestigkeit of 85.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
360.0 °C | 47.0 MPa Show Material materials with Zugfestigkeit of 47.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | ||
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
100.0 °C | 2.39e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.39e-05 1/K | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 610.0 - 640.0 °C Show Material materials with Schmelzpunkt of 610.0 - 640.0 °C | O | EN 573-3, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
Spezifische Wärmekapazität | 20.0 °C | 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 963.0 J/(kg·K) | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Wärmeleitfähigkeit | 20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 23000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
spezifischer Widerstand | 4.35e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 5e-08 Ω·m | O | EN 573-3, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 Show Material materials with Chrom of 0.3 | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
0.40 % Show Material materials with Eisen of 0.40 % | O | EN 573-3, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Magnesium | 2.6 - 3.6 % Show Material materials with Magnesium of 2.6 - 3.6 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good to good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |