Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H14 | EN 573-3, EN 1592, EN 485, EN 754 | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3, EN 485, EN 754 | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3, EN 754 | A100 | |||
4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3, EN 485 | A50 | |||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | A100 | |||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | A50 | |||
7.0 % Show Material materials with Dehnung of 7.0 % | H14 | EN 573-3, EN 1592 | A100 | |||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | A10 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3, EN 1592, EN 485, EN 754 | |||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube | ||
Härte, Brinell | 72.0 [-] Show Material materials with Härte, Brinell of 72.0 [-] | H14 | EN 573-3, EN 485 | |||
75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | H14 | EN 573-3, EN 754 | ||||
20.0 °C | 73.0 [-] Show Material materials with Härte, Brinell of 73.0 [-] | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 26.5 Show Material materials with Schubmodule of 26.5 | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube | |
Zugfestigkeit | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H14 | EN 573-3, EN 1592 | |||
240.0 - 290.0 MPa Show Material materials with Zugfestigkeit of 240.0 - 290.0 MPa | H14 | EN 573-3, EN 754 | ||||
20.0 °C | 240.0 - 280.0 MPa Show Material materials with Zugfestigkeit of 240.0 - 280.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Sheet, Strip | ||
20.0 °C | 250.0 MPa Show Material materials with Zugfestigkeit of 250.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H14 | EN 573-3, EN 1592, EN 485, EN 754 | ||
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H14 | EN 573-3, EN 1592, EN 485, EN 754 | |||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube | Long | |
150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||||
Schmelzpunkt | 620.0 - 650.0 °C Show Material materials with Schmelzpunkt of 620.0 - 650.0 °C | H14 | EN 573-3, EN 1592, EN 485, EN 754 | |||
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 140.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 180.0 W/(m·K) | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 25000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 25000000.0 S/m | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
spezifischer Widerstand | 4e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4e-08 - 5e-08 Ω·m | H14 | EN 573-3, EN 1592, EN 485, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube |
0.50 % Show Material materials with Eisen of 0.50 % | H14 | EN 573-3, EN 1592, EN 485, EN 754 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Magnesium | 1.6 - 2.5 % Show Material materials with Magnesium of 1.6 - 2.5 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Mangan | 0.5 - 1.1 % Show Material materials with Mangan of 0.5 - 1.1 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |