DIN 1712-3 Grade 3.0255 O

View suppliers (9)
Want to keep this datasheet? Save it now in your required format

Description

Pure aluminium This material is well anodically oxidizable, and possesses a good electrical and thermal conductivity. The splinter-giving workability is bad because of danger of smearing. Its mechanical strength is low, the plasticity high. The forming capacity and the chemical as well as the weather proofness are excellent. The material is well suitable for welding and braze welding. Application: apparatus engineering, roll bond, z-bond, household devices, camp and transportation containers for the chemical, pharmaceutical and food industry, roofings, linings, arts and crafts, packing, flow pressed parts (tubes, tube, doses, bottles), reflectors, generally metal-describe, large bottles (to 10 l), metal goods, far neck catches, heat exchanger (profiles, gilled pipes), pressure tanks according to AD-W 6/1, liquid air separation, thermal insulation, antennas, parabolic reflector, tank -, silo trucks, body parts, aircraft construction, tools, forms and devices in mechanical engineering.

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM,AluKey zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValueConditionRelated StandardsShape

Dichte

2.7 g/cm³

Show Material materials with Dichte of 2.7 g/cm³

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

20.0 °C

2.7 g/cm³

Show Material materials with Dichte of 2.7 g/cm³

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

Mechanisch

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

25.0 MPa

Show Material materials with Bending Fatigue Strength of 25.0 MPa

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Biegewinkel 180°

0.5 °/t

Show Material materials with Biegewinkel 180° of 0.5 °/t

O

EN 573-3, EN 485

1.0 °/t

Show Material materials with Biegewinkel 180° of 1.0 °/t

O

EN 573-3, EN 485

Biegewinkel 90°

0.5 °/t

Show Material materials with Biegewinkel 90° of 0.5 °/t

O

EN 573-3, EN 485

1.0 °/t

Show Material materials with Biegewinkel 90° of 1.0 °/t

O

EN 573-3, EN 485

Dehnung

1.0 %

Show Material materials with Dehnung of 1.0 %

O

EN 573-3, EN 546

A50

2.0 %

Show Material materials with Dehnung of 2.0 %

O

EN 573-3, EN 546

A50

4.0 %

Show Material materials with Dehnung of 4.0 %

O

EN 573-3, EN 546

A50

6.0 %

Show Material materials with Dehnung of 6.0 %

O

EN 573-3, EN 546, EN 683

A50

10.0 %

Show Material materials with Dehnung of 10.0 %

O

EN 573-3, EN 546, EN 683

A50

15.0 %

Show Material materials with Dehnung of 15.0 %

O

EN 573-3, EN 683

A50

20.0 %

Show Material materials with Dehnung of 20.0 %

O

EN 573-3, EN 1396, EN 485

A50

22.0 %

Show Material materials with Dehnung of 22.0 %

O

EN 573-3, EN 1396, EN 485, EN 754

A50

23.0 %

Show Material materials with Dehnung of 23.0 %

O

EN 573-3, EN 755

A50

25.0 %

Show Material materials with Dehnung of 25.0 %

O

EN 573-3, EN 754, EN 755

A100

26.0 %

Show Material materials with Dehnung of 26.0 %

O

EN 573-3, EN 1396, EN 485

A50

29.0 %

Show Material materials with Dehnung of 29.0 %

O

EN 573-3, EN 485

A50

32.0 %

Show Material materials with Dehnung of 32.0 %

O

EN 573-3, EN 485

A100

35.0 %

Show Material materials with Dehnung of 35.0 %

O

EN 573-3, EN 1301

35.0 %

Show Material materials with Dehnung of 35.0 %

O

EN 573-3, EN 485

A50

20.0 °C

5.0 %

Show Material materials with Dehnung of 5.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Flat

A100

20.0 °C

8.0 %

Show Material materials with Dehnung of 8.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Flat

A100

20.0 °C

10.0 %

Show Material materials with Dehnung of 10.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Flat

A100

20.0 °C

15.0 %

Show Material materials with Dehnung of 15.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Flat

A100

20.0 °C

18.0 %

Show Material materials with Dehnung of 18.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A100

20.0 °C

22.0 %

Show Material materials with Dehnung of 22.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A10

20.0 °C

23.0 %

Show Material materials with Dehnung of 23.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Tube

A10

20.0 °C

27.0 %

Show Material materials with Dehnung of 27.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Tube

20.0 °C

30.0 %

Show Material materials with Dehnung of 30.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Flat

A10

20.0 °C

35.0 %

Show Material materials with Dehnung of 35.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip

A10

20.0 °C

35.0 %

Show Material materials with Dehnung of 35.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Sheet

20.0 °C

40.0 %

Show Material materials with Dehnung of 40.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Strip, Sheet

Elastizitätsmodul

-195.0 °C

78.4 GPa

Show Material materials with Elastizitätsmodul of 78.4 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

-85.0 °C

73.5 GPa

Show Material materials with Elastizitätsmodul of 73.5 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

-30.0 °C

71.4 GPa

Show Material materials with Elastizitätsmodul of 71.4 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

69.0 GPa

Show Material materials with Elastizitätsmodul of 69.0 GPa

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastizitätsmodul of 60.0 - 70.0 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

20.0 °C

70.0 GPa

Show Material materials with Elastizitätsmodul of 70.0 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

100.0 °C

68.6 GPa

Show Material materials with Elastizitätsmodul of 68.6 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

150.0 °C

66.5 GPa

Show Material materials with Elastizitätsmodul of 66.5 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

200.0 °C

63.0 GPa

Show Material materials with Elastizitätsmodul of 63.0 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

250.0 °C

56.0 GPa

Show Material materials with Elastizitätsmodul of 56.0 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

Härte, Brinell

20.0 [-]

Show Material materials with Härte, Brinell of 20.0 [-]

O

EN 573-3, EN 485

20.0 °C

20.0 [-]

Show Material materials with Härte, Brinell of 20.0 [-]

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Strip, Tube, Wire, Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poissonzahl

0.33 [-]

Show Material materials with Poissonzahl of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Schubmodule

25.9 GPa

Show Material materials with Schubmodule of 25.9 GPa

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Schubmodule of 25.0 - 26.5 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

Zugfestigkeit

35.0 - 80.0 MPa

Show Material materials with Zugfestigkeit of 35.0 - 80.0 MPa

O

EN 573-3, EN 546

40.0 - 85.0 MPa

Show Material materials with Zugfestigkeit of 40.0 - 85.0 MPa

O

EN 573-3, EN 546

45.0 - 95.0 MPa

Show Material materials with Zugfestigkeit of 45.0 - 95.0 MPa

O

EN 573-3, EN 546

45.0 - 90.0 MPa

Show Material materials with Zugfestigkeit of 45.0 - 90.0 MPa

O

EN 573-3, EN 546

50.0 - 95.0 MPa

Show Material materials with Zugfestigkeit of 50.0 - 95.0 MPa

O

EN 573-3, EN 546, EN 683

60.0 - 80.0 MPa

Show Material materials with Zugfestigkeit of 60.0 - 80.0 MPa

O

EN 573-3, EN 1715-3

60.0 MPa

Show Material materials with Zugfestigkeit of 60.0 MPa

O

EN 573-3, EN 755

95.0 MPa

Show Material materials with Zugfestigkeit of 95.0 MPa

O

EN 573-3, EN 1301

20.0 °C

55.0 - 90.0 MPa

Show Material materials with Zugfestigkeit of 55.0 - 90.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Flat

20.0 °C

55.0 - 95.0 MPa

Show Material materials with Zugfestigkeit of 55.0 - 95.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Flat

20.0 °C

60.0 MPa

Show Material materials with Zugfestigkeit of 60.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

20.0 °C

60.0 - 90.0 MPa

Show Material materials with Zugfestigkeit of 60.0 - 90.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Flat

20.0 °C

60.0 - 95.0 MPa

Show Material materials with Zugfestigkeit of 60.0 - 95.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4, EN 754, EN 755

Flat

20.0 °C

65.0 MPa

Show Material materials with Zugfestigkeit of 65.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Tube

20.0 °C

65.0 - 95.0 MPa

Show Material materials with Zugfestigkeit of 65.0 - 95.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4, EN 1396, EN 485

Strip, Sheet, Flat

Thermisch

PropertyTemperatureValueConditionRelated StandardsShape

Koeffizient der thermischen Ausdehnung

-50 °C

2.17e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

-50.0 °C

2.17e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

20 °C

2.17e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

20 °C

2.35e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

100 °C

2.35e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

100.0 °C

2.35e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

200.0 °C

2.44e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.44e-05 1/K

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

300.0 °C

2.54e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.54e-05 1/K

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

Schmelzpunkt

646.0 - 657.0 °C

Show Material materials with Schmelzpunkt of 646.0 - 657.0 °C

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Spezifische Wärmekapazität

900.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K)

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

20.0 °C

900.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K)

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

Wärmeleitfähigkeit

20.0 °C

210.0 - 220.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 210.0 - 220.0 W/(m·K)

O

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Rod, Sheet, Flat, Strip, Tube, Wire

Elektrisch

PropertyTemperatureValueConditionRelated StandardsShape

Elektrische Leitfähigkeit

34000000.0 - 36000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 34000000.0 - 36000000.0 S/m

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

20.0 °C

34800000.0 - 36000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 34800000.0 - 36000000.0 S/m

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

spezifischer Widerstand

2.78e-08 - 2.94e-08 Ω·m

Show Material materials with spezifischer Widerstand of 2.78e-08 - 2.94e-08 Ω·m

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Eisen

0.4 %

Show Material materials with Eisen of 0.4 %

O

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Flat, Strip, Tube, Wire

0.40 %

Show Material materials with Eisen of 0.40 %

O

EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Kupfer

0.05 %

Show Material materials with Kupfer of 0.05 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Rod, Sheet, Flat, Strip, Tube, Wire

Magnesium

0.05 %

Show Material materials with Magnesium of 0.05 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Rod, Sheet, Flat, Strip, Tube, Wire

Mangan

0.05 %

Show Material materials with Mangan of 0.05 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Rod, Sheet, Flat, Strip, Tube, Wire

Silizium

0.25 %

Show Material materials with Silizium of 0.25 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Rod, Sheet, Flat, Strip, Tube, Wire

Titan

0.05 %

Show Material materials with Titan of 0.05 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Rod, Sheet, Flat, Strip, Tube, Wire

Zink

0.07 %

Show Material materials with Zink of 0.07 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755

Rod, Sheet, Flat, Strip, Tube, Wire

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: acceptable, weathering: good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12)