Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.75 - 2.8 g/cm³ Show Material materials with Dichte of 2.75 - 2.8 g/cm³ | Typical for Cast 2xx.x Series Aluminium |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastizitätsmodul | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | Typical for Cast 2xx.x Series Aluminium | |||
Härte, Brinell | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T4 | Pink Sheets, ASTM B108 | Casting | |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 2xx.x Series Aluminium | |||
Zugfestigkeit | 230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | T4 | Pink Sheets, ASTM B108 | Casting |
Thermisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1.9e-05 - 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9e-05 - 2.3e-05 1/K | Typical for Cast 2xx.x Series Aluminium | |||
Schmelzpunkt | 521.0 - 632.0 °C Show Material materials with Schmelzpunkt of 521.0 - 632.0 °C | T4 | Pink Sheets, ASTM B108 | Casting | |
Spezifische Wärmekapazität | 875.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 875.0 - 963.0 J/(kg·K) | Typical for Cast 2xx.x Series Aluminium | |||
Wärmeleitfähigkeit | 120.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 - 150.0 W/(m·K) | Typical for Cast 2xx.x Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 16000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 23000000.0 S/m | Typical for Cast 2xx.x Series Aluminium |
spezifischer Widerstand | 4.347826086956522e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.347826086956522e-08 - 6.25e-08 Ω·m | Typical for Cast 2xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 1.20 % Show Material materials with Eisen of 1.20 % | T4 | Pink Sheets, ASTM B108 | Casting |
Kupfer | 4.0 - 5.0 % Show Material materials with Kupfer of 4.0 - 5.0 % | T4 | Pink Sheets, ASTM B108 | Casting |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | T4 | Pink Sheets, ASTM B108 | Casting |
Mangan | 0.35 % Show Material materials with Mangan of 0.35 % | T4 | Pink Sheets, ASTM B108 | Casting |
Nickel | 0.35 % Show Material materials with Nickel of 0.35 % | T4 | Pink Sheets, ASTM B108 | Casting |
Silizium | 2.0 - 3.0 % Show Material materials with Silizium of 2.0 - 3.0 % | T4 | Pink Sheets, ASTM B108 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T4 | Pink Sheets, ASTM B108 | Casting |
Zink | 0.5 % Show Material materials with Zink of 0.5 % | T4 | Pink Sheets, ASTM B108 | Casting |