Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.65 - 2.7 g/cm³ Show Material materials with Dichte of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastizitätsmodul | 73.0 - 80.0 GPa Show Material materials with Elastizitätsmodul of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Härte, Brinell | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
95.0 [-] Show Material materials with Härte, Brinell of 95.0 [-] | F | Pink Sheets, ASTM B108 | Casting | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Zugfestigkeit | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | F | Pink Sheets, ASTM B108 | Casting |
Thermisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.3e-05 1/K | Typical for Cast 3xx.x Series Aluminium | |||
Schmelzpunkt | 510.0 - 607.0 °C Show Material materials with Schmelzpunkt of 510.0 - 607.0 °C | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting | |
Spezifische Wärmekapazität | 960.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | |||
Wärmeleitfähigkeit | 130.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 180.0 W/(m·K) | Typical for Cast 3xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 1.00 % Show Material materials with Eisen of 1.00 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Kupfer | 3.0 - 4.0 % Show Material materials with Kupfer of 3.0 - 4.0 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Nickel | 0.35 % Show Material materials with Nickel of 0.35 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Silizium | 5.5 - 6.5 % Show Material materials with Silizium of 5.5 - 6.5 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Zink | 1.0 % Show Material materials with Zink of 1.0 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |