Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A50 | 23.0 °C | 5 - 12 % Show Material materials with Dehnung A50 of 5 - 12 % | |
Elastizitätsmodul | 23.0 °C | 96 - 120 GPa Show Material materials with Elastizitätsmodul of 96 - 120 GPa | Typical for Cast Copper Bronze |
Poissonzahl | 23.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] | Typical for Cast Copper Bronze |
Streckgrenze Rp0,5 | 23.0 °C | 97 - 110 MPa Show Material materials with Streckgrenze Rp0,5 of 97 - 110 MPa | |
Zugfestigkeit | 23.0 °C | 172 - 179 MPa Show Material materials with Zugfestigkeit of 172 - 179 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.6E-5 - 1.9E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 - 1.9E-5 1/K | Typical for Cast Copper Bronze |
Schmelzpunkt | 760 - 1060 °C Show Material materials with Schmelzpunkt of 760 - 1060 °C | Typical for Cast Copper Bronze | |
Spezifische Wärmekapazität | 23.0 °C | 376 - 440 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 376 - 440 J/(kg·K) | Typical for Cast Copper Bronze |
Wärmeleitfähigkeit | 23.0 °C | 12 - 81 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 12 - 81 W/(m·K) | Typical for Cast Copper Bronze |
Chemical properties
Property | Value |
---|---|
Aluminium | 5E-3 % Show Material materials with Aluminium of 5E-3 % |
Antimon | 0.5 - 0.8 % Show Material materials with Antimon of 0.5 - 0.8 % |
Blei | 13 - 16 % Show Material materials with Blei of 13 - 16 % |
Eisen | 0.1 - 0.15 % Show Material materials with Eisen of 0.1 - 0.15 % |
Kupfer | 75 - 79 % Show Material materials with Kupfer of 75 - 79 % |
Nickel | 0.8 - 1 % Show Material materials with Nickel of 0.8 - 1 % |
Phosphor | 0.05 - 1.5 % Show Material materials with Phosphor of 0.05 - 1.5 % |
Schwefel | 0.08 % Show Material materials with Schwefel of 0.08 % |
Silizium | 5E-3 % Show Material materials with Silizium of 5E-3 % |
Zink | 0.8 % Show Material materials with Zink of 0.8 % |
Zinn | 6.3 - 7.5 % Show Material materials with Zinn of 6.3 - 7.5 % |