Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 8.9 g/cm³ Show Material materials with Dichte of 8.9 g/cm³ | Typical for Wrought Copper Pure / Low Alloyed Copper |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 23.0 °C | 95 - 98 GPa Show Material materials with Elastizitätsmodul of 95 - 98 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Poissonzahl | 23.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] | Typical for Wrought Copper Pure / Low Alloyed Copper |
Schubmodule | 23.0 °C | 48 GPa Show Material materials with Schubmodule of 48 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.6E-5 - 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 - 1.8E-5 1/K | Typical for Wrought Copper Pure / Low Alloyed Copper |
Schmelzpunkt | 965 - 1100 °C Show Material materials with Schmelzpunkt of 965 - 1100 °C | Typical for Wrought Copper Pure / Low Alloyed Copper | |
Spezifische Wärmekapazität | 23.0 °C | 377 - 420 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 377 - 420 J/(kg·K) | Typical for Wrought Copper Pure / Low Alloyed Copper |
Chemical properties
Property | Value |
---|---|
Andere | total 0.05, Cu+Ag > 99.85 |
Antimon | 5E-3 % Show Material materials with Antimon of 5E-3 % |
Arsen | 0.02 % Show Material materials with Arsen of 0.02 % |
Bismut | 3E-3 % Show Material materials with Bismut of 3E-3 % |
Blei | 0.01 % Show Material materials with Blei of 0.01 % |
Eisen | 0.01 % Show Material materials with Eisen of 0.01 % |
Nickel | 0.05 % Show Material materials with Nickel of 0.05 % |
Sauerstoff | 0.1 % Show Material materials with Sauerstoff of 0.1 % |
Selen | 0.2 % Show Material materials with Selen of 0.2 % |
Tellur | 0.01 % Show Material materials with Tellur of 0.01 % |
Zinn | 0.01 % Show Material materials with Zinn of 0.01 % |