Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.9 g/cm³ Show Material materials with Dichte of 8.9 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 23.0 °C | 30 % Show Material materials with Dehnung of 30 % | |
Elastizitätsmodul | 23.0 °C | 110 GPa Show Material materials with Elastizitätsmodul of 110 GPa | |
Poissonzahl | 23.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] | Typical for Wrought Copper Pure / Low Alloyed Copper |
Schubmodule | 23.0 °C | 48 GPa Show Material materials with Schubmodule of 48 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20.0 °C | 1.77E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.77E-5 1/K | |
100.0 °C | 1.77E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.77E-5 1/K | ||
Schmelzpunkt | 1083 °C Show Material materials with Schmelzpunkt of 1083 °C | ||
Spezifische Wärmekapazität | 23.0 °C | 377 - 420 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 377 - 420 J/(kg·K) | Typical for Wrought Copper Pure / Low Alloyed Copper |
Wärmeleitfähigkeit | 23.0 °C | 386 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 386 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 23.0 °C | 5.70E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 5.70E+7 S/m |
spezifischer Widerstand | 23.0 °C | 1.75E-8 Ω·m Show Material materials with spezifischer Widerstand of 1.75E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Andere | total 0.03. excluded Ag, P |
Bismut | 5E-4 % Show Material materials with Bismut of 5E-4 % |
Blei | 5E-3 % Show Material materials with Blei of 5E-3 % |
Kupfer | 99.95 % Show Material materials with Kupfer of 99.95 % |
Phosphor | 2E-3 - 7E-3 % Show Material materials with Phosphor of 2E-3 - 7E-3 % |
Selen | 2E-4 % Show Material materials with Selen of 2E-4 % |
Technological properties
Property | ||
---|---|---|
Brazing | hard brazing : very good, soft brazing: very good | |
Workability | Cold forming degree between anneals: max. 95 %, general (condition): very good |