Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 6.7 g/cm³ Show Material materials with Dichte of 6.7 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Bending Fatigue Strength | 23.0 °C | 48 MPa Show Material materials with Bending Fatigue Strength of 48 MPa | |
Dehnung | 20.0 °C | 3 % Show Material materials with Dehnung of 3 % | |
80.0 °C | 10 % Show Material materials with Dehnung of 10 % | ||
150.0 °C | 21 % Show Material materials with Dehnung of 21 % | ||
Dehnung A50 | 20.0 °C | 10 % Show Material materials with Dehnung A50 of 10 % | |
23.0 °C | 10 % Show Material materials with Dehnung A50 of 10 % | ||
Elastizitätsmodul | 20.0 °C | 85 GPa Show Material materials with Elastizitätsmodul of 85 GPa | |
Härte, Brinell | 20.0 °C | 80 - 83 [-] Show Material materials with Härte, Brinell of 80 - 83 [-] | |
23.0 °C | 83 [-] Show Material materials with Härte, Brinell of 83 [-] | ||
80.0 °C | 55 [-] Show Material materials with Härte, Brinell of 55 [-] | ||
150.0 °C | 28 [-] Show Material materials with Härte, Brinell of 28 [-] | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Zinc Aluminium |
Streckgrenze Rp 0,2 | 20.0 °C | 200 - 220 MPa Show Material materials with Streckgrenze Rp 0,2 of 200 - 220 MPa | |
23.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 0,2 of 200 MPa | ||
80.0 °C | 160 MPa Show Material materials with Streckgrenze Rp 0,2 of 160 MPa | ||
150.0 °C | 70 MPa Show Material materials with Streckgrenze Rp 0,2 of 70 MPa | ||
Zugfestigkeit | 20.0 °C | 275 - 280 MPa Show Material materials with Zugfestigkeit of 275 - 280 MPa | |
23.0 °C | 280 MPa Show Material materials with Zugfestigkeit of 280 MPa | ||
80.0 °C | 222 MPa Show Material materials with Zugfestigkeit of 222 MPa | ||
150.0 °C | 140 MPa Show Material materials with Zugfestigkeit of 140 MPa | ||
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 2.2E-5 - 2.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2E-5 - 2.8E-5 1/K | Typical for Zinc Aluminium |
Schmelzpunkt | 375 - 485 °C Show Material materials with Schmelzpunkt of 375 - 485 °C | Typical for Zinc Aluminium | |
Spezifische Wärmekapazität | 23.0 °C | 393 - 525 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 393 - 525 J/(kg·K) | Typical for Zinc Aluminium |
Wärmeleitfähigkeit | 20.0 °C | 113 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 113 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.51E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 1.51E+7 S/m |
spezifischer Widerstand | 20.0 °C | 6.6E-8 Ω·m Show Material materials with spezifischer Widerstand of 6.6E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 3.7 - 4.3 % Show Material materials with Aluminium of 3.7 - 4.3 % |
Andere | Rest Zn |
Blei | 5E-3 % Show Material materials with Blei of 5E-3 % |
Cadmium | 5E-3 % Show Material materials with Cadmium of 5E-3 % |
Eisen | 0.05 % Show Material materials with Eisen of 0.05 % |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % |
Magnesium | 0.03 - 0.06 % Show Material materials with Magnesium of 0.03 - 0.06 % |
Nickel | 0.02 % Show Material materials with Nickel of 0.02 % |
Silizium | 0.03 % Show Material materials with Silizium of 0.03 % |
Zink | 95.43 % Show Material materials with Zink of 95.43 % |
Zinn | 2E-3 % Show Material materials with Zinn of 2E-3 % |