Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.8 g/cm³ Show Material materials with Dichte of 8.8 g/cm³ |
Abmessung
Property | Value |
---|---|
Dimensions | Durchmesser |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 35 % Show Material materials with Dehnung of 35 % |
Elastizitätsmodul | 20.0 °C | 143 GPa Show Material materials with Elastizitätsmodul of 143 GPa |
Elongation A100 | 20.0 °C | 25 % Show Material materials with Elongation A100 of 25 % |
Härte, Brinell | 20.0 °C | 50 - 75 [-] Show Material materials with Härte, Brinell of 50 - 75 [-] |
Härte, Vickers | 20.0 °C | 55 - 80 [-] Show Material materials with Härte, Vickers of 55 - 80 [-] |
Streckgrenze Rp 0,2 | 20.0 °C | 90 MPa Show Material materials with Streckgrenze Rp 0,2 of 90 MPa |
Zugfestigkeit | 20.0 °C | 240 MPa Show Material materials with Zugfestigkeit of 240 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 20.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K |
100.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | |
Schmelzpunkt | 1050 - 1070 °C Show Material materials with Schmelzpunkt of 1050 - 1070 °C | |
Wärmeleitfähigkeit | 20.0 °C | 75 - 126 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 75 - 126 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.10E+7 - 2.40E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 1.10E+7 - 2.40E+7 S/m |
spezifischer Widerstand | 20.0 °C | 4.17E-8 - 9.09E-8 Ω·m Show Material materials with spezifischer Widerstand of 4.17E-8 - 9.09E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Andere | Rest Cu, total 0.3 |
Blei | 0.02 % Show Material materials with Blei of 0.02 % |
Eisen | 0.2 % Show Material materials with Eisen of 0.2 % |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % |
Nickel | 1 - 1.6 % Show Material materials with Nickel of 1 - 1.6 % |
Silizium | 0.4 - 0.7 % Show Material materials with Silizium of 0.4 - 0.7 % |
Technological properties
Property | ||
---|---|---|
Brazing | hard brazing : good to medium, soft brazing: good | |
Workability | Cold forming degree between anneals: max. 75 % (lösungsgeglüht) |