Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 2.68 g/cm³ Show Supplier Material materials with Dichte of 2.68 g/cm³ |
Mechanisch
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 2.4E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2.4E-5 1/K | 20-100°C |
Wärmeleitfähigkeit | 23.0 °C | 168 - 190 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 168 - 190 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 23.0 °C | 3.5E-8 Ω·m Show Supplier Material materials with spezifischer Widerstand of 3.5E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Andere | 0.05 - 0.15 % Show Supplier Material materials with Andere of 0.05 - 0.15 % |
Chrom | 0.1 % Show Supplier Material materials with Chrom of 0.1 % |
Eisen | 0.45 % Show Supplier Material materials with Eisen of 0.45 % |
Kupfer | 0.05 % Show Supplier Material materials with Kupfer of 0.05 % |
Magnesium | 0.7 - 1.1 % Show Supplier Material materials with Magnesium of 0.7 - 1.1 % |
Mangan | 0.15 % Show Supplier Material materials with Mangan of 0.15 % |
Silizium | 0.3 % Show Supplier Material materials with Silizium of 0.3 % |
Zink | 0.2 % Show Supplier Material materials with Zink of 0.2 % |
Technological properties
Property | ||
---|---|---|
Anodizing | Excellent (anodizing quality) | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Heat exchangers: Fins; Cosmetics: Cosmetics pieces; Pharmacy: Pharma and para-Pharma; Automotive Trim: Interior Trim, Windows frames; Components: Automotive fins, Heat exchangers | |
Brazing | Good | |
Corrosion properties | Excellent | |
Welding | Excellent | |
Workability | Good |