Allgemein
Property | Temperature | Value | |
---|---|---|---|
Dichte | 23.0 °C | 14 g/cm³ Show Supplier Material materials with Dichte of 14 g/cm³ | |
Binder | Cobalt binder | ||
Kornstruktur | Fine grain size |
Mechanisch
Property | Temperature | Value |
---|---|---|
Druckfestigkeit | 23.0 °C | 4000 MPa Show Supplier Material materials with Druckfestigkeit of 4000 MPa |
Elastizitätsmodul | 23.0 °C | 530 GPa Show Supplier Material materials with Elastizitätsmodul of 530 GPa |
Härte, Rockwell A | 23.0 °C | 87.8 [-] Show Supplier Material materials with Härte, Rockwell A of 87.8 [-] |
Härte, Vickers, 10 | 23.0 °C | 1150 [-] Show Supplier Material materials with Härte, Vickers, 10 of 1150 [-] |
Plane-Strain Fracture Toughnes | 23.0 °C | 14.3 MPa·√m Show Supplier Material materials with Plane-Strain Fracture Toughnes of 14.3 MPa·√m |
Zugfestigkeit, transversal | 23.0 °C | 2900 MPa Show Supplier Material materials with Zugfestigkeit, transversal of 2900 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 6.5E-6 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 6.5E-6 1/K |
Wärmeleitfähigkeit | 23.0 °C | 90 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 90 W/(m·K) |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Kobalt | 15 % Show Supplier Material materials with Kobalt of 15 % | as binder | |
Wolfram | WC balance |
Technological properties
Property |
---|