Allgemein
Property | Value |
---|---|
Carbon equivalent note | Typical values for carbon equivalent (CEV) can be submitted upon request. |
Mechanisch
Property | Temperature | Value | Testing Standard | Comment |
---|---|---|---|---|
Charpy impact energy, V-notch | -40 °C | 24 J Show Supplier Material materials with Charpy impact energy, V-notch of 24 J | EN ISO 148-1 | average of 3 tests for basic grade | longitudinal and transverse specimens |
-40 °C | 32 J Show Supplier Material materials with Charpy impact energy, V-notch of 32 J | EN ISO 148-1 | average of 3 tests for extra tough grade | longitudinal and transverse specimens | |
Dehnung | 8 % Show Supplier Material materials with Dehnung of 8 % | EN ISO 6892-1 | min. for plate thickness 6 < t ≤ 80 mm | transverse specimens, A5 | |
Härte, Brinell | 480 - 530 [-] Show Supplier Material materials with Härte, Brinell of 480 - 530 [-] | HBW | ||
Streckgrenze | 1250 MPa Show Supplier Material materials with Streckgrenze of 1250 MPa | EN ISO 6892-1 | min. Rp0.2 for plate thickness 40 < t ≤ 80 mm | transverse specimens | |
1300 MPa Show Supplier Material materials with Streckgrenze of 1300 MPa | EN ISO 6892-1 | min. Rp0.2 for plate thickness 6 < t ≤ 40 mm | transverse specimens | ||
Zugfestigkeit | 1450 MPa Show Supplier Material materials with Zugfestigkeit of 1450 MPa | EN ISO 6892-1 | min. for plate thickness 40 < t ≤ 80 mm | transverse specimens | |
1500 MPa Show Supplier Material materials with Zugfestigkeit of 1500 MPa | EN ISO 6892-1 | min. for plate thickness 6 < t ≤ 40 mm | transverse specimens |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Chrom | 2 % Show Supplier Material materials with Chrom of 2 % | max. | |
Eisen | Balance | ||
Kohlenstoff | 0.32 % Show Supplier Material materials with Kohlenstoff of 0.32 % | max. | |
Mangan | 1.2 % Show Supplier Material materials with Mangan of 1.2 % | max. | |
Molybdän | 0.7 % Show Supplier Material materials with Molybdän of 0.7 % | max. | |
Nickel | 3.7 % Show Supplier Material materials with Nickel of 3.7 % | max. | |
Phosphor | 0.015 % Show Supplier Material materials with Phosphor of 0.015 % | max. | |
Schwefel | 0.005 % Show Supplier Material materials with Schwefel of 0.005 % | max. | |
Silizium | 0.5 % Show Supplier Material materials with Silizium of 0.5 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | It is preferably used for light weight armoured vehicles. Due to its performance the steel is used by the customers for civil and military protection systems. | |
Cold Forming | The material can be formed by cold bending, in spite of its high hardness. It is recommended that the thermal cutting or shearing edges in the area of the bend should be grinded. The bending speed must be adjusted by the fabricator to the geometry of the processed parts. Due to the high strength values of DIFENDER 500 in the quenched and tempered condition the spring-back phenomenon has to be taken into account while cold forming. During the processing, the necessary safety measures have to be taken, so that nobody will be exposed to a danger by a possible fracture of the work piece during the forming process. | |
Delivery condtion | The plates are delivered in the quenched and tempered condition. DIFENDER 500 can be delivered in two grades as follows: | |
General note | If particular requirements, which are not covered in this material data sheet, are to be met by the steel due to its intended use or processing, these requirements are to be agreed before placing the order. The information in this technical data sheet is a product description. This material data sheet is updated at irregular intervals. The current version is available from the mill or as download at www.dillinger.de. | |
Heat Treatment | DIFENDER 500 is delivered in a heat treatment condition which is ready for assembly. Subsequent heat treatment above 200 °C impairs its ballistic properties and is therefore not permissible. | |
Machining | DIFENDER 500 is suitable for machining. In view of its high delivery hardness a lower cutting speed must be anticipated. | |
Other | DIFENDER 500 can be supplied in the following dimensions: On request, other dimensions can be agreed. | |
Processing methods | The entire processing and application techniques are of fundamental importance to the reliability of the products made from this steel. The user should ensure that his design, construction and processing methods are aligned with the material, correspond to the state-of-the-art that the fabricator has to comply with and are suitable for the intended use. The customer is responsible for the selection of the material. The recommendations in accordance with EN 1011 should be observed. The much higher tensile properties of the armoured steel comparing to other steels covered by the standard can lead to a higher crack probability while processing. | |
Properties under ballistic impacts | The properties under ballistic impacts have to be agreed. | |
Surface condition | Surface quality: Unless otherwise agreed, the indications in accordance with EN 10163-2, class A3, apply. Higher requirements may be agreed upon request. | |
Surface protection | Surface protection Upon request the plates can be shot blasted and / or primer coated with a product at the manufacturer’s choice. In case you wish the application of a shop primer, but you do not specify the shop primer in detail, Dillinger offers shop primers as standard: you will find more information in our brochure „Shot blasted and primer coated heavy plates“ (www.dillinger.de) | |
Testings | Ultrasonic testing: Unless otherwise agreed, indications be in accordance with EN 10160, class S2/E2 apply. p>Determination of the mechanical properties in the delivery condition per plate as rolled in 1⁄4 plate width in accordance with ISO 404. The hardness test is carried out in accordance with ISO 6506-1. The tensile test is carried out on flat rectangular, transverse specimens in accordance with EN ISO 6892-1. The impact test will be carried out on Charpy-V-longitudinal and transverse specimens in accordance with EN ISO 148-1. The test results are documented in a certificate 3.1 in accordance with EN 10204. A bullet resistance test can be agreed upon. Tensile testing on transverse specimens at room temperature | |
Thermal cutting and welding | The heat input during welding and thermal cutting can lead to a decrease in hardness in a small area adjacent to or in the weld seam. This can have an impact on the bullet resistance properties of DIFENDER 500. The manufacturer is advised to take this into account in his design. | |
Tolerances | Unless otherwise agreed the following tolerances apply: For width and length tolerances EN 10029 table 2 and 3 will apply. Smaller flatness tolerances may be agreed upon request. |