Mechanisch
Property | Value | Comment |
---|---|---|
Härte, Brinell | 150 - 220 [-] Show Supplier Material materials with Härte, Brinell of 150 - 220 [-] | HBW | delivery condition |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1.11e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.11e-05 1/K | 20-100 °C | |
1.18e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.18e-05 1/K | 20-200 °C | ||
1.28e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.28e-05 1/K | 20-300 °C | ||
1.36e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | 20-400 °C | ||
1.37e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.37e-05 1/K | 20-500 °C | ||
1.43e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.43e-05 1/K | 20-600 °C | ||
Spezifische Wärmekapazität | 470 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 470 J/(kg·K) | ||
Wärmeleitfähigkeit | 20 °C | 48 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 48 W/(m·K) | |
100 °C | 49 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 49 W/(m·K) | ||
200 °C | 49 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 49 W/(m·K) | ||
300 °C | 48 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 48 W/(m·K) | ||
400 °C | 47 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 47 W/(m·K) |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Andere | 0.09 % Show Supplier Material materials with Andere of 0.09 % | auxiliary data | |
0.63 % Show Supplier Material materials with Andere of 0.63 % | max. limiting values for Cr+Mo+Ni for steel grades according DIN EN 10083-2 | ||
Chrom | 0.04 % Show Supplier Material materials with Chrom of 0.04 % | auxiliary data | |
0.4 % Show Supplier Material materials with Chrom of 0.4 % | max. limiting values for steel grades according DIN EN 10083-2 | ||
Eisen | Balance | ||
Kohlenstoff | 0.42 - 0.5 % Show Supplier Material materials with Kohlenstoff of 0.42 - 0.5 % | limiting values | |
0.47 % Show Supplier Material materials with Kohlenstoff of 0.47 % | auxiliary data | ||
Mangan | 0.5 - 0.8 % Show Supplier Material materials with Mangan of 0.5 - 0.8 % | limiting values | |
0.74 % Show Supplier Material materials with Mangan of 0.74 % | auxiliary data | ||
Molybdän | 0.09 % Show Supplier Material materials with Molybdän of 0.09 % | auxiliary data | |
0.1 % Show Supplier Material materials with Molybdän of 0.1 % | max. limiting values for steel grades according DIN EN 10083-2 | ||
Nickel | 0.04 % Show Supplier Material materials with Nickel of 0.04 % | auxiliary data | |
0.4 % Show Supplier Material materials with Nickel of 0.4 % | max. limiting values for steel grades according DIN EN 10083-2 | ||
Phosphor | 0.017 % Show Supplier Material materials with Phosphor of 0.017 % | auxiliary data | |
0.025 % Show Supplier Material materials with Phosphor of 0.025 % | max. limiting values | ||
Schwefel | 0.002 % Show Supplier Material materials with Schwefel of 0.002 % | auxiliary data | |
0.01 % Show Supplier Material materials with Schwefel of 0.01 % | max. limiting values | ||
Silizium | 0.34 % Show Supplier Material materials with Silizium of 0.34 % | auxiliary data | |
0.4 % Show Supplier Material materials with Silizium of 0.4 % | max. limiting values |
Technological properties
Property | ||
---|---|---|
Application areas | DIMO C45 is designed for holderblock applications requiring extensive machining and high dimensional stability as mold assemblies, ejector plates, supports, clamping plates and housings for diecasting dies. | |
Delivery condtion | DIMO C45 is supplied in a stress relieved condition with a normalized ferrite-pearlite-microstructure. The normalizing can be replaced by a normalizing rolling. Cut edges are stress relieved by an appropriate heat treatment. | |
General note | If special requirements, which are not listed in this specification, are to be met by the steel due to its intended use or processing, these requirements are to be agreed before placing the order. The information in this specification is a product description. This specification is updated if necessary. The latest version is available from the mill or as download at www.dillinger.de. | |
Heat Treatment | DIMOC45 is generally applied in the delivery condition. Should a heat treatment become necessary, please refer to the material data sheet at www.dillinger.de. | |
Other | DIMO C45 is available as plate with cut edges (sheared, flame cut or water jet cut) in the following dimensions: Widths < 1500 mm (59 in) have to be ordered with an even number of plates, Other dimensions available upon request. | |
Processing history | The DIMO C45 production route is designed to achieve good machinability, dimensional stability and high cleanliness. The good oxidic cleanliness and the modification of remaining inclusions by the calcium treatment lead to good machinability and minimize the tool wear. These properties can only be achieved by the combination of the following DIMO C45-production steps: | |
Surface condition | Surface quality: Unless otherwise agreed, the specifications will be in accordance with EN 10163-2 class A, subclass 3. Shot blasting of upper and lower surface of the plate and shop priming are possible on request. | |
Testings | Unless otherwise agreed, the results are documented in an inspection certificate 3.1 in accordance with EN 10204. | |
Tolerances | Unless otherwise agreed, tolerances are in accordance with EN 10029 with the following restrictions: |