Allgemein
Property | Temperature | Value | Testing Standard |
---|---|---|---|
Dichte | 25 °C | 1.04 g/cm³ Show Supplier Material materials with Dichte of 1.04 g/cm³ | ISO 1183-1 |
Mechanisch
Property | Temperature | Value | Testing Standard | Comment |
---|---|---|---|---|
Biegefestigkeit | 62 MPa Show Supplier Material materials with Biegefestigkeit of 62 MPa | ISO 178 | 2 mm/min | |
Biegemodul | 2.1 GPa Show Supplier Material materials with Biegemodul of 2.1 GPa | ISO 527-1/2 | 2 mm/min | |
Dehnung | 15 % Show Supplier Material materials with Dehnung of 15 % | ISO 527-1/2 | min. | 50 mm/min | |
Elastizitätsmodul | 2.3 GPa Show Supplier Material materials with Elastizitätsmodul of 2.3 GPa | ISO 527-1/2 | 1 mm/min | |
Elongation at yield | 2.1 % Show Supplier Material materials with Elongation at yield of 2.1 % | ISO 527-1/2 | 50 mm/min | |
Hardness, Ball Indentation | 95 MPa Show Supplier Material materials with Hardness, Ball Indentation of 95 MPa | ISO 2039-1 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 11 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 11 kJ/m² | ISO 179-1eA | |
23 °C | 22 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 22 kJ/m² | ISO 179-1eA | ||
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 120 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 120 kJ/m² | ISO 179-1eU | |
23 °C | 180 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 180 kJ/m² | ISO 179-1eU | ||
Schlagzähigkeit, Izod gekerbt | -30 °C | 11 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 11 kJ/m² | ISO 180-1A | |
23 °C | 23 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 23 kJ/m² | ISO 180-1A | ||
Streckgrenze | 39 MPa Show Supplier Material materials with Streckgrenze of 39 MPa | ISO 527-1/2 | 50 mm/min |
Thermisch
Property | Value | Testing Standard | Pressure | Comment | |||
---|---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 0.0001 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 0.0001 1/K | ISO 11359-1/2 | 23 to 55°C | ||||
Vicat-Erweichungstemperatur | 98 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 98 °C | ISO 306 | 50 N | 50°C/h | ||||
Wärmeformbeständigkeitstemperatur | 93 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 93 °C | ISO 75-1/2 | 1.8 MPa | ||||
97 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 97 °C | ISO 75-1/2 | 0.45 MPa | |||||
Entflammbarkeit | At thickness 1.6 mm UL 94: HB. Burning rate US-FMVSS (200x105x2 mm): 55 mm/min according to ISO 3795 |
Elektrisch
Property | Value | Frequency | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3 [-] | 1MHz | IEC 60250 | |
3.1 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.1 [-] | 100Hz | IEC 60250 | ||
Durchschlagfestigkeit | 33 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 33 kV/mm | IEC 60243-1 | 1 mm | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | IEC 60112 | Solution A | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | |||
Verlustfaktor | 0.006 [-] Show Supplier Material materials with Verlustfaktor of 0.006 [-] | 100Hz | IEC 60250 | |
0.008 [-] Show Supplier Material materials with Verlustfaktor of 0.008 [-] | 1MHz | IEC 60250 | ||
Volume resistivity | 1e+15 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+15 Ω·cm | IEC 60093 |
Rheological Properties
Property | Value | Testing Standard | Comment |
---|---|---|---|
Schmelzvolumenflussrate | 22 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 22 cm³/10min | ISO 1133 | 220°C/10Kg |
Schrumpfung | 0.4 - 0.7 % Show Supplier Material materials with Schrumpfung of 0.4 - 0.7 % | ISO 2577 | 60x60x2 |
0.4 - 0.7 % Show Supplier Material materials with Schrumpfung of 0.4 - 0.7 % | ISO 2577 | 60x60x2, Transverse |
Technological properties
Property | ||
---|---|---|
Certifications | UL Certificate | |
Handling recommendations | Please see the Material Safety Data Sheet for relevant health & safety information. | |
Other | Control measurements in other places may issue different results due to influences of machinery, equipment, test method or storage conditions. | |
Processing methods | Injection molding-melt temperature: 240 ºC according to ISO 294 Injection molding-mold temperature: 70 ºC according to ISO 294 Injection molding-injection velocity: 240 mm/s according to ISO 294 |