Stabar K200 Polyetheretherketone Polymer Film (EK301075)

Alternative und Handelsbezeichungen
Stabar K200 Polyetheretherketone Polymer Film (EK301075)
Want to keep this datasheet? Save it now in your required format

Description

PEEK is an inherently crystalline polymer with a high crystalline melting point of 340 °C, but “Stabar” K200 film has been manufactured in such a way that full crystallinity has not been developed in the film. The result is that “Stabar” K200 is a highly transparent low haze film and has the ability to be thermoformed and embossed at temperature below 200 °C.


Heat treatment of “Stabar” K200 film between its melting point and the glass transition temperature of 143 °C will induce crystallisation as seen by the onset of opacity, higher rigidity at high temperatures, and improved solvent resistance.

Diese Materialdaten wurden von Matmatch zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

Eigenschaften

Allgemein

PropertyTemperatureValueComment

Koeffizient hygroskopischer Ausdehnung

23.0 °C

5E-6 %

Show Material materials with Koeffizient hygroskopischer Ausdehnung of 5E-6 %

Permeabilitätskoeffizient

23.0 °C

13 cm²/s

Show Material materials with Permeabilitätskoeffizient of 13 cm²/s

E96

Sauerstoffindex

23.0 °C

25 %

Show Material materials with Sauerstoffindex of 25 %

D2863-77

Wasserabsorption

23.0 °C

0.4 %

Show Material materials with Wasserabsorption of 0.4 %

24h

Mechanisch

PropertyTemperatureValueComment

Dehnung

23.0 °C

240 %

Show Material materials with Dehnung of 240 %

D882-67

Dehnung, transversal

23.0 °C

240 %

Show Material materials with Dehnung, transversal of 240 %

D882-67

Zugfestigkeit

23.0 °C

120 MPa

Show Material materials with Zugfestigkeit of 120 MPa

D882-67

Zugfestigkeit, transversal

23.0 °C

120 MPa

Show Material materials with Zugfestigkeit, transversal of 120 MPa

D882-67

Thermisch

PropertyTemperatureValue

Glasübergangstemperatur

143 °C

Show Material materials with Glasübergangstemperatur of 143 °C

Koeffizient der thermischen Ausdehnung

110.0 °C

4E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 4E-5 1/K

Max. Betriebstemperatur, lang

250 °C

Show Material materials with Max. Betriebstemperatur, lang of 250 °C

Spezifische Wärmekapazität

23.0 °C

1450 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 1450 J/(kg·K)

Entflammbarkeit

UL94 VTM -1 (100 micron)

Elektrisch

PropertyTemperatureValueComment

Dielektrizitätskonstante

25.0 °C

3.3 [-]

Show Material materials with Dielektrizitätskonstante of 3.3 [-]

at 50Hz, D150

Dissipation factor, 50Hz

25.0 °C

1.8E-3 [-]

Show Material materials with Dissipation factor, 50Hz of 1.8E-3 [-]

D150

100.0 °C

1.6E-3 [-]

Show Material materials with Dissipation factor, 50Hz of 1.6E-3 [-]

D150

Durchschlagfestigkeit

23.0 °C

128 kV/mm

Show Material materials with Durchschlagfestigkeit of 128 kV/mm

D194-64

spezifischer Widerstand

25.0 °C

1.00E+15 Ω·m

Show Material materials with spezifischer Widerstand of 1.00E+15 Ω·m

D257

Rheological Properties

PropertyTemperatureValueComment

Schrumpfung

150.0 °C

0.5 %

Show Material materials with Schrumpfung of 0.5 %

30s

Schrumpfung, diagonal

150.0 °C

0.5 %

Show Material materials with Schrumpfung, diagonal of 0.5 %

30s

Technological properties

Property
Other

“Stabar” K200 film offers an excellent combination of properties including: Intrinsic long term heat stability; Low flammability and extremely low smoke and toxic gas evolution on burning; Resistance to attack by a wide range of organic and inorganic chemicals and solvents; Low water absorption and good hydrolysis resistance at high temperatures and pressures; Resistance to radiation (X-rays, beta-rays and gamma rays) is amongst the best of thermoplastic materials; Good tear and fatigue resistance; Retention of good electrical properties over a wide temperature range.

Processing methods

“Stabar” K200 film can be adhesion-bonded either to itself or to other substrates, the bond strengths being dependent upon the type of adhesive and the surface preparation. “Stabar” K200 film may be fusion- bonded to itself, to reinforcements and to other substrates by application of heat and pressure. “Stabar” K200 film can be metallised by vacuum deposition and sputtering techniques, and is compatible with a range of inks and lacquers.