Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.46 g/cm³ Show Supplier Material materials with Dichte of 1.46 g/cm³ | ASTM D792 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 338 MPa Show Supplier Material materials with Biegefestigkeit of 338 MPa | ASTM D790 |
Biegemodul | 23.0 °C | 11.72 GPa Show Supplier Material materials with Biegemodul of 11.72 GPa | ASTM D790 |
Dehnung | 23.0 °C | 2 - 3 % Show Supplier Material materials with Dehnung of 2 - 3 % | ASTM D638 |
Elastizitätsmodul | 23.0 °C | 19.79 GPa Show Supplier Material materials with Elastizitätsmodul of 19.79 GPa | ASTM D638 |
Impact strength, Izod notched, ASTM | 23.0 °C | 320 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 320 J/m | ASTM D256 |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 1121 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 1121 J/m | ASTM D4812 |
Zugfestigkeit | 23.0 °C | 228 MPa Show Supplier Material materials with Zugfestigkeit of 228 MPa | ASTM D638 |
Thermisch
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 254 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 254 °C | ASTM D648 | |
Entflammbarkeit | HB ASTM D635, for 1.5mm |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schrumpfung | 23.0 °C | 0.1 - 0.3 % Show Supplier Material materials with Schrumpfung of 0.1 - 0.3 % | ASTM D955, (1/8 in (3.2 mm)section) |
Technological properties
Property | ||
---|---|---|
Application areas | Suitable for automotive (Spare wheel pan, Door module, Dashboard cross member, Seat pan, Bumper bracket, Front end), electronic appliances, sport equipment, power tools, tool handles, high speed rail accessories and etc. | |
Fillers | 43% Long Glass Fiber | |
Processing methods | Injection Moulding. Injection Pressure 34 - 124 MPa, Melt Temperature 271 - 299 °C, Mould temperature 66 - 124 °C, Pre-drying 2-4 hrs @ 79 °C, Moisture Content 0.2%, Dew Point -18°C |