Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.17 g/cm³ Show Material materials with Dichte of 1.17 g/cm³ | ASTM D 792 |
Wasserabsorption | 23.0 °C | 0.1 % Show Material materials with Wasserabsorption of 0.1 % | ASTM D 570 | 24 Hours |
Wasseraufnahme, Gleichgewicht | 23.0 °C | 0.4 % Show Material materials with Wasseraufnahme, Gleichgewicht of 0.4 % | ASTM D 570 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegemodul | 23.0 °C | 2.68 GPa Show Material materials with Biegemodul of 2.68 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Dehnung | 23.0 °C | 50 % Show Material materials with Dehnung of 50 % | ASTM D 638 | Type I, 50 mm/min |
Elastizitätsmodul | 23.0 °C | 2.68 GPa Show Material materials with Elastizitätsmodul of 2.68 GPa | ASTM D 638 | 50 mm/min |
Elongation at yield | 23.0 °C | 5 % Show Material materials with Elongation at yield of 5 % | ASTM D 638 | Type I, 50 mm/min |
Flexural yield strength | 23.0 °C | 96 MPa Show Material materials with Flexural yield strength of 96 MPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Hardness, Rockwell R | 23.0 °C | 120 [-] Show Material materials with Hardness, Rockwell R of 120 [-] | ASTM D 785 |
Impact strength, Izod notched, ASTM | 23.0 °C | 427 J/m Show Material materials with Impact strength, Izod notched, ASTM of 427 J/m | ASTM D 256 |
Streckgrenze | 23.0 °C | 58 MPa Show Material materials with Streckgrenze of 58 MPa | ASTM D 638 | Type I, 50 mm/min |
Thermisch
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Heat deflection temperature, 1.80 MPa | 80 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 80 °C | ASTM D 648 | 1.82 MPa, 6.4 mm, unannealed | |||
Koeffizient der thermischen Ausdehnung | 23.0 °C | 7.2E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.2E-5 1/K | ASTM E 831 | -40°C to 60°C | ||
Relative temperature index, electrical | 80 °C Show Material materials with Relative temperature index, electrical of 80 °C | UL 746B | |||
Relative temperature index, mechanical impact | 70 °C Show Material materials with Relative temperature index, mechanical impact of 70 °C | UL 746B | |||
Relative temperature index, mechanical strength | 80 °C Show Material materials with Relative temperature index, mechanical strength of 80 °C | UL 746B | |||
Vicat-Erweichungstemperatur | 90 °C Show Material materials with Vicat-Erweichungstemperatur of 90 °C | ASTM D 1525 | Rate B/50 | |||
Wärmeleitfähigkeit | 23.0 °C | 0.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 0.2 W/(m·K) | ASTM C177 | ||
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 7.2E-5 1/K Show Material materials with thermischer Ausdehnungskoeffizient, transversal of 7.2E-5 1/K | ASTM E 831 | -40°C to 60°C | ||
Entflammbarkeit | UL Recognized, 94-5VB Flame Class Rating | 2.31mm | UL 94 |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dielektrizitätskonstante | 23.0 °C | 3 [-] Show Material materials with Dielektrizitätskonstante of 3 [-] | ASTM D 150 | at 100 Hz |
Durchschlagfestigkeit | 23.0 °C | 17.9 kV/mm Show Material materials with Durchschlagfestigkeit of 17.9 kV/mm | ASTM D 149 | in oil, 3.2 mm |
Kriechstromfestigkeit | 23.0 °C | 1 V Show Material materials with Kriechstromfestigkeit of 1 V | UL 746A |
Verlustfaktor | 23.0 °C | 4.8E-3 [-] Show Material materials with Verlustfaktor of 4.8E-3 [-] | ASTM D 150 | at 50/60 Hz |
spezifischer Widerstand | 23.0 °C | 1.00E+15 Ω·m Show Material materials with spezifischer Widerstand of 1.00E+15 Ω·m | ASTM D 257 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzmassenflussrate | 16 g/10min Show Material materials with Schmelzmassenflussrate of 16 g/10min | ASTM D 1238 | 260°C/2.16 kgf | |
Schrumpfung | 23.0 °C | 0.4 - 0.6 % Show Material materials with Schrumpfung of 0.4 - 0.6 % | SABIC method | 3.2 mm |
Schrumpfung, diagonal | 23.0 °C | 0.4 - 0.6 % Show Material materials with Schrumpfung, diagonal of 0.4 - 0.6 % | SABIC method |
Technological properties
Property | ||
---|---|---|
Application areas | Air Conditioning,Amusement Machine,ATM/Ticket Machine,Audio,Building Accessory,Circuit Protection,Data Management,Data Transfer,Dishwasher,Displays,Document Handling,Electronic Components,Enclosure/Housing/Cover,Enclosures,Energy Management,Freezer,Furnace/Heater,Heavy Vehicles,Infotainment/Telematic,Lab Ware and Clinical Diagnostics,Laundry Dryer,LED Lighting,Medical Device,Meter Gas,Monitoring and Imaging,Non-LED Lighting,Personal Computing,Pharmaceutical Packaging & Drug Delivery,Power Manangement,Refrigerator,Sail Boat,Security/Detection,Small Appliance,Surgical Tray,Trim,Vacuum Cleaner,Vending Machine,Washing Machine,Wearables,Wireless Communications,Wiring Devices | |
Processing methods | Drying Temperature: 75-80°C, Drying Time: 3-4hrs, Drying Time (Cumulative): 8hrs, Maximum Moisture Content: 0.04%, Melt Temperature: 230-275°C, Nozzle Temperature: 230-275°C, Front - Zone 3 Temperature: 225-275°C, Middle - Zone 2 Temperature: 215-260°C, Rear - Zone 1 Temperature: 210-255°C, Mold Temperature: 50-70°C, Back Pressure: 0.3-0.7MPa, Screw Speed: 40-70rpm, Shot to Cylinder Size: 30-80%, Vent Depth: 0.038-0.076mm |