Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.04 g/cm³ Show Material materials with Dichte of 1.04 g/cm³ | ASTM D 792 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegemodul | 23.0 °C | 2.4 GPa Show Material materials with Biegemodul of 2.4 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Dehnung | 23.0 °C | 42.9 % Show Material materials with Dehnung of 42.9 % | ASTM D 638 | Type I, 5 mm/min |
Elastizitätsmodul | 23.0 °C | 2.13 GPa Show Material materials with Elastizitätsmodul of 2.13 GPa | ASTM D 638 | 5 mm/min |
Elongation at yield | 23.0 °C | 2.4 % Show Material materials with Elongation at yield of 2.4 % | ASTM D 638 | Type I, 5 mm/min |
Flexural yield strength | 23.0 °C | 73 MPa Show Material materials with Flexural yield strength of 73 MPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Impact strength, Izod notched, ASTM | 23.0 °C | 421 J/m Show Material materials with Impact strength, Izod notched, ASTM of 421 J/m | ASTM D 256 |
Streckgrenze | 23.0 °C | 39 MPa Show Material materials with Streckgrenze of 39 MPa | ASTM D 638 | Type I, 5 mm/min |
Zugfestigkeit | 23.0 °C | 33 MPa Show Material materials with Zugfestigkeit of 33 MPa | ASTM D 638 | Type I, 5 mm/min |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 82 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 82 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |
Koeffizient der thermischen Ausdehnung | 23.0 °C | 7.92E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.92E-5 1/K | ASTM E 831 | -40°C to 40°C |
Vicat-Erweichungstemperatur | 106 °C Show Material materials with Vicat-Erweichungstemperatur of 106 °C | ASTM D 1525 | Rate B/50 | |
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 8.1E-5 1/K Show Material materials with thermischer Ausdehnungskoeffizient, transversal of 8.1E-5 1/K | ASTM E 831 | -40°C to 40°C |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Melt viscosity | 23.0 °C | 1160 Pa·s Show Material materials with Melt viscosity of 1160 Pa·s | ASTM D 3825 | 240°C, 100 sec⁻¹ |
Schmelzvolumenflussrate | 9 cm³/10min Show Material materials with Schmelzvolumenflussrate of 9 cm³/10min | ISO 1133 | 220°C/10.0 kg | |
Schrumpfung | 23.0 °C | 0.5 - 0.7 % Show Material materials with Schrumpfung of 0.5 - 0.7 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Building/Construction Sheet | |
Processing methods | Drying Temperature: 90-95°C, Drying Time (Cumulative): 4hrs, Maximum Moisture Content: 0%, Melt Temperature: 200-220°C, Barrel - Zone 1 Temperature: 170-190°C, Barrel - Zone 2 Temperature: 180-200°C, Barrel - Zone 3 Temperature: 175-205°C, Barrel - Zone 4 Temperature: 180-210°C, Adapter Temperature: 180-205°C, Die Temperature: 180-215°C |