Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.31 g/cm³ Show Material materials with Dichte of 1.31 g/cm³ | ASTM D 792 |
Wasserabsorption | 23.0 °C | 0.08 % Show Material materials with Wasserabsorption of 0.08 % | ISO 62 | 23°C, 50% RH |
Mechanisch
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Biegemodul | 23.0 °C | 2.4 GPa Show Material materials with Biegemodul of 2.4 GPa | ISO 178 | 2 mm/min | ||
Dehnung | 23.0 °C | 25 % Show Material materials with Dehnung of 25 % | ASTM D 638 | Type I, 50 mm/min | ||
Elastizitätsmodul | 23.0 °C | 2.5 GPa Show Material materials with Elastizitätsmodul of 2.5 GPa | ASTM D 638 | 50 mm/min | ||
Elongation at yield | 23.0 °C | 6 % Show Material materials with Elongation at yield of 6 % | ASTM D 638 | Type I, 50 mm/min | ||
Flexural yield strength | 23.0 °C | 85 MPa Show Material materials with Flexural yield strength of 85 MPa | ISO 178 | 2 mm/min | ||
Impact strength, Izod notched, ASTM | -30.0 °C | 53 J/m Show Material materials with Impact strength, Izod notched, ASTM of 53 J/m | ASTM D 256 | ||
23.0 °C | 53 J/m Show Material materials with Impact strength, Izod notched, ASTM of 53 J/m | ASTM D 256 | |||
Schlagfestigkeit, Charpy gekerbt | -30.0 °C | 2 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 2 kJ/m² | ISO 179/1eA | ||
23.0 °C | 3 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 3 kJ/m² | ISO 179/1eA | |||
Schlagzähigkeit, Izod gekerbt | -30.0 °C | 3 kJ/m² Show Material materials with Schlagzähigkeit, Izod gekerbt of 3 kJ/m² | ISO 180/1A | ||
23.0 °C | 3 kJ/m² Show Material materials with Schlagzähigkeit, Izod gekerbt of 3 kJ/m² | ISO 180/1A | |||
Streckgrenze | 23.0 °C | 51 MPa Show Material materials with Streckgrenze of 51 MPa | ASTM D 638 | Type I, 50 mm/min | ||
Zugfestigkeit | 23.0 °C | 30 MPa Show Material materials with Zugfestigkeit of 30 MPa | ASTM D 638 | Type I, 50 mm/min | ||
Schlagzähigkeit, Charpy ungekerbt | No Break @ 23,-30°C | ISO 179/1eU | ||||
Schlagzähigkeit, Izod ungekerbt | No Break @ 23,-30°C| ISO 180/1U |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 54 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 54 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1E-4 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-4 1/K | ASTM E 831 | -40°C to 40°C |
Vicat-Erweichungstemperatur | 175 °C Show Material materials with Vicat-Erweichungstemperatur of 175 °C | ASTM D 1525 | Rate B/50 | |
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 1E-4 1/K Show Material materials with thermischer Ausdehnungskoeffizient, transversal of 1E-4 1/K | ASTM E 831 | -40°C to 40°C |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzmassenflussrate | 35 g/10min Show Material materials with Schmelzmassenflussrate of 35 g/10min | ASTM D 1238 | 250°C/1.2 kgf | |
Schmelzvolumenflussrate | 31 cm³/10min Show Material materials with Schmelzvolumenflussrate of 31 cm³/10min | ISO 1133 | 250°C/1.2 kg | |
Schrumpfung | 23.0 °C | 0.9 - 1.6 % Show Material materials with Schrumpfung of 0.9 - 1.6 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Bottles,Medical Device,Pharmaceutical Packaging & Drug Delivery | |
Processing methods | Drying Temperature: 110-120°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 250-270°C, Nozzle Temperature: 240-260°C, Front - Zone 3 Temperature: 245-265°C, Middle - Zone 2 Temperature: 240-255°C, Rear - Zone 1 Temperature: 230-245°C, Hopper Temperature: 40-60°C, Mold Temperature: 40-100°C |