Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.23 g/cm³ Show Material materials with Dichte of 1.23 g/cm³ | ASTM D 792 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 82 MPa Show Material materials with Biegefestigkeit of 82 MPa | ASTM D 790 |
Biegemodul | 23.0 °C | 2.15 GPa Show Material materials with Biegemodul of 2.15 GPa | ASTM D 790 |
Dehnung | 23.0 °C | 200 % Show Material materials with Dehnung of 200 % | SABIC - Japan Method |
Impact strength, Izod notched, ASTM | -30.0 °C | 50 J/m Show Material materials with Impact strength, Izod notched, ASTM of 50 J/m | ASTM D 256 |
23.0 °C | 392 J/m Show Material materials with Impact strength, Izod notched, ASTM of 392 J/m | ASTM D 256 | |
Streckgrenze | 23.0 °C | 52 MPa Show Material materials with Streckgrenze of 52 MPa | SABIC - Japan Method |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 130 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 130 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |
Koeffizient der thermischen Ausdehnung | 23.0 °C | 6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 6E-5 1/K | TMA | -30°C to 30°C |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schrumpfung | 23.0 °C | 0.5 - 0.8 % Show Material materials with Schrumpfung of 0.5 - 0.8 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Displays,Document Handling,Door Handle,Electronic Components,Exterior,Front Grille,Rear/Signal Lighting,Recreational Vehicle,Security/Detection |