Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.34 g/cm³ Show Material materials with Dichte of 1.34 g/cm³ | ISO 1183 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 170 MPa Show Material materials with Biegefestigkeit of 170 MPa | ISO 178 |
Biegemodul | 23.0 °C | 6.5 GPa Show Material materials with Biegemodul of 6.5 GPa | ISO 178 |
Dehnung | 23.0 °C | 2.5 % Show Material materials with Dehnung of 2.5 % | ISO 527-1/-2 |
Elastizitätsmodul | 23.0 °C | 7.5 GPa Show Material materials with Elastizitätsmodul of 7.5 GPa | ISO 527-1/-2 |
Poissonzahl | 23.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] | |
Schlagfestigkeit, Charpy gekerbt | -6.0 °C | 8 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | ISO 179/1eA |
23.0 °C | 8.5 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 8.5 kJ/m² | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -6.0 °C | 45 kJ/m² Show Material materials with Schlagzähigkeit, Charpy ungekerbt of 45 kJ/m² | ISO 179/1eU |
23.0 °C | 50 kJ/m² Show Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | ISO 179/1eU | |
Schlagzähigkeit, Izod gekerbt | -40.0 °C | 45 kJ/m² Show Material materials with Schlagzähigkeit, Izod gekerbt of 45 kJ/m² | ISO 180/1U |
23.0 °C | 45 kJ/m² Show Material materials with Schlagzähigkeit, Izod gekerbt of 45 kJ/m² | ISO 180/1U | |
Schlagzähigkeit, Izod ungekerbt | -40.0 °C | 7 kJ/m² Show Material materials with Schlagzähigkeit, Izod ungekerbt of 7 kJ/m² | ISO 180/1A |
-30.0 °C | 7 kJ/m² Show Material materials with Schlagzähigkeit, Izod ungekerbt of 7 kJ/m² | ISO 180/1A | |
23.0 °C | 7 kJ/m² Show Material materials with Schlagzähigkeit, Izod ungekerbt of 7 kJ/m² | ISO 180/1A | |
Zugfestigkeit | 23.0 °C | 120 MPa Show Material materials with Zugfestigkeit of 120 MPa | ISO 527-1/-2 |
Thermisch
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Glasübergangstemperatur | 110 °C Show Material materials with Glasübergangstemperatur of 110 °C | ISO 11357-1/-2 | 18°F/min | |||
Heat deflection temperature, 1.80 MPa | 175 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 175 °C | ISO 75-1/-2 | |||
Koeffizient der thermischen Ausdehnung | 23.0 °C | 3E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 3E-5 1/K | ISO 11359-1/-2 | ||
Relative temperature index, electrical | 130 °C Show Material materials with Relative temperature index, electrical of 130 °C | UL 746B | 120mil | |||
Relative temperature index, mechanical impact | 130 °C Show Material materials with Relative temperature index, mechanical impact of 130 °C | UL 746B | 120mil | |||
Relative temperature index, mechanical strength | 130 °C Show Material materials with Relative temperature index, mechanical strength of 130 °C | UL 746B | 120mil | |||
Schmelzpunkt | 220 °C Show Material materials with Schmelzpunkt of 220 °C | ISO 11357-1/-3 | 18°F/min | |||
Spezifische Wärmekapazität | 23.0 °C | 1900 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 1900 J/(kg·K) | of melt | ||
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 1E-4 1/K Show Material materials with thermischer Ausdehnungskoeffizient, transversal of 1E-4 1/K | ISO 11359-1/-2 | ||
Entflammbarkeit | Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: HB class, Thickness tested: 0.75 mm, UL recognition: yes -, FMVSS Class: B -, Burning rate, Thickness 1 mm: 31 mm/min |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Kriechstromfestigkeit | 23.0 °C | 500 V Show Material materials with Kriechstromfestigkeit of 500 V | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzvolumenflussrate | 15 cm³/10min Show Material materials with Schmelzvolumenflussrate of 15 cm³/10min | ISO 1133 | |
Schrumpfung | 23.0 °C | 0.4 % Show Material materials with Schrumpfung of 0.4 % | ISO 294-4, 2577 |
Schrumpfung, diagonal | 23.0 °C | 0.7 % Show Material materials with Schrumpfung, diagonal of 0.7 % | ISO 294-4, 2577 |
Technological properties
Property | ||
---|---|---|
Fillers | 20% Glass Fiber | |
Processing methods | Drying Recommended: yes, Drying Temperature: 120°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.04%, Melt Temperature Optimum: 250°C, Min. melt temperature: 240°C, Max. melt temperature: 260°C, Mold Temperature Optimum: 80°C, Min. mold temperature: 30°C, Max. mold temperature: 130°C, Hold pressure range: ≥60MPa, Hold pressure time: 3s/mm, Back pressure: As low as possible, Ejection temperature: 170°C |