Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.83 g/cm³ Show Material materials with Dichte of 1.83 g/cm³ | ISO 1183 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 23.0 °C | 1.6 % Show Material materials with Dehnung of 1.6 % | ISO 527-1/-2 |
Elastizitätsmodul | 23.0 °C | 12.6 GPa Show Material materials with Elastizitätsmodul of 12.6 GPa | ISO 527-1/-2 |
Poissonzahl | 23.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | |
Schlagfestigkeit, Charpy gekerbt | 23.0 °C | 10 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 10 kJ/m² | ISO 179/1eA |
Schlagzähigkeit, Charpy ungekerbt | 23.0 °C | 36 kJ/m² Show Material materials with Schlagzähigkeit, Charpy ungekerbt of 36 kJ/m² | ISO 179/1eU |
Zugfestigkeit | 23.0 °C | 129 MPa Show Material materials with Zugfestigkeit of 129 MPa | ISO 527-1/-2 |
Thermisch
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 218 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 218 °C | ISO 75-1/-2 | |
Relative temperature index, electrical | 155 °C Show Material materials with Relative temperature index, electrical of 155 °C | UL 746B | 120mil | |
Relative temperature index, mechanical impact | 155 °C Show Material materials with Relative temperature index, mechanical impact of 155 °C | UL 746B | 120mil | |
Relative temperature index, mechanical strength | 155 °C Show Material materials with Relative temperature index, mechanical strength of 155 °C | UL 746B | 120mil | |
Schmelzpunkt | 247 °C Show Material materials with Schmelzpunkt of 247 °C | ISO 11357-1/-3 | 18°F/min | |
Entflammbarkeit | Burning Behav. at 60mil nom. thickn.: V-0 class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: V-0 class, Thickness tested: 0.75 mm, UL recognition: yes -, Burning Behav. 5V at thickness h: 5VA class, Thickness tested: 2 mm, UL recognition: yes -, Glow Wire Flammability Index, 30mil: 960 °C, Glow Wire Flammability Index, 60mil: 960 °C, Glow Wire Flammability Index, 80mil: 960 °C, Glow Wire Flammability Index, 120mil: 960 °C, Glow Wire Ignition Temperature, 30mil: 900 °C, Glow Wire Ignition Temperature, 60mil: 900 °C, Glow Wire Ignition Temperature, 80mil: 900 °C, Glow Wire Ignition Temperature, 120mil: 875 °C, Glow Wire Temperature, No Flame, 40mil: 850 °C, Glow Wire Temperature, No Flame, 80mil: 800 °C, FMVSS Class: DNI - |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dielektrizitätskonstante, 1 MHz | 23.0 °C | 4.3 [-] Show Material materials with Dielektrizitätskonstante, 1 MHz of 4.3 [-] | IEC 62631-2-1 |
Dielektrizitätskonstante, 100 Hz | 23.0 °C | 4.6 [-] Show Material materials with Dielektrizitätskonstante, 100 Hz of 4.6 [-] | IEC 62631-2-1 |
Dissipation factor, 100Hz | 23.0 °C | 4.4E-3 [-] Show Material materials with Dissipation factor, 100Hz of 4.4E-3 [-] | IEC 62631-2-1 |
Dissipation factor, 1MHz | 23.0 °C | 0.01 [-] Show Material materials with Dissipation factor, 1MHz of 0.01 [-] | IEC 62631-2-1 |
Durchschlagfestigkeit | 23.0 °C | 34 kV/mm Show Material materials with Durchschlagfestigkeit of 34 kV/mm | IEC 60243-1 |
Kriechstromfestigkeit | 23.0 °C | 2 V Show Material materials with Kriechstromfestigkeit of 2 V | UL 746A |
Surface resistivity | 23.0 °C | 1.00E+13 Ω/sq Show Material materials with Surface resistivity of 1.00E+13 Ω/sq | IEC 62631-3-2 |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Material materials with Volume resistivity of 1.00E+15 Ω·cm | min. | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Fillers | 45% Glass Fiber and Mineral Powder | |
Processing methods | Drying Recommended: yes, Drying Temperature: 120°C, Drying Time, Dehumidified Dryer: 4-6h, Processing Moisture Content: ≤0.02%, Melt Temperature Optimum: 280°C, Min. melt temperature: 270°C, Max. melt temperature: 290°C, Max. screw tangential speed: 0.2m/s, Mold Temperature Optimum: 110°C, Min. mold temperature: 100°C, Max. mold temperature: 120°C, Hold pressure range: ≥80MPa, Hold pressure time: 4s/mm, Back pressure: As low as possible, Ejection temperature: 170°C |