Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.16 g/cm³ Show Material materials with Dichte of 1.16 g/cm³ | ISO 1183 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegemodul | 23.0 °C | 0.27 GPa Show Material materials with Biegemodul of 0.27 GPa | ISO 178 |
Dehnung | 23.0 °C | 300 % Show Material materials with Dehnung of 300 % | ISO 527-1/-2 |
Elastizitätsmodul | 23.0 °C | 0.27 GPa Show Material materials with Elastizitätsmodul of 0.27 GPa | ISO 527-1/-2 |
Härte, Shore D | 23.0 °C | 60 [-] Show Material materials with Härte, Shore D of 60 [-] | max., ISO 7619-1 |
Poissonzahl | 23.0 °C | 0.48 [-] Show Material materials with Poissonzahl of 0.48 [-] | |
Reißfestigkeit | 23.0 °C | 140 kN/m Show Material materials with Reißfestigkeit of 140 kN/m | ISO 34-1 |
Reißfestigkeit, transversal | 23.0 °C | 130 kN/m Show Material materials with Reißfestigkeit, transversal of 130 kN/m | ISO 34-1 |
Schlagfestigkeit, Charpy gekerbt | -40.0 °C | 7 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 7 kJ/m² | ISO 179/1eA |
-6.0 °C | 12 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 12 kJ/m² | ISO 179/1eA | |
23.0 °C | 102 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 102 kJ/m² | ISO 179/1eA | |
Schlagzähigkeit, Izod ungekerbt | -40.0 °C | 7 kJ/m² Show Material materials with Schlagzähigkeit, Izod ungekerbt of 7 kJ/m² | ISO 180/1A |
Zugfestigkeit | 23.0 °C | 33 MPa Show Material materials with Zugfestigkeit of 33 MPa | ISO 527-1/-2 |
Thermisch
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Brittleness temperature | -65 °C Show Material materials with Brittleness temperature of -65 °C | ISO 974 | |||
Glasübergangstemperatur | 15 °C Show Material materials with Glasübergangstemperatur of 15 °C | ISO 11357-1/-2 | 18°F/min | |||
Heat deflection temperature, 0.45 MPa | 65 °C Show Material materials with Heat deflection temperature, 0.45 MPa of 65 °C | ISO 75-1/-2 | |||
Heat deflection temperature, 1.80 MPa | 45 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 45 °C | ISO 75-1/-2 | |||
Koeffizient der thermischen Ausdehnung | 23.0 °C | 2E-4 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2E-4 1/K | ISO 11359-1/-2 | -40 - 23°C | ||
Schmelzpunkt | 215 °C Show Material materials with Schmelzpunkt of 215 °C | ISO 11357-1/-3 | 18°F/min | |||
Vicat-Erweichungstemperatur | 195 °C Show Material materials with Vicat-Erweichungstemperatur of 195 °C | ISO 306 | 90°F, 2 lbf | |||
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 1.8E-4 1/K Show Material materials with thermischer Ausdehnungskoeffizient, transversal of 1.8E-4 1/K | ISO 11359-1/-2 | -40 - 23°C | ||
Entflammbarkeit | FMVSS Class: B -, Burning rate, Thickness 1 mm: <80 mm/min |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzmassenflussrate | 4 g/10min Show Material materials with Schmelzmassenflussrate of 4 g/10min | ISO 1133 | 240°C/10kg | |
Schrumpfung | 23.0 °C | 2.4 % Show Material materials with Schrumpfung of 2.4 % | ISO 294-4, 2577 |
Schrumpfung, diagonal | 23.0 °C | 2.2 % Show Material materials with Schrumpfung, diagonal of 2.2 % | ISO 294-4, 2577 |
Technological properties
Property |
---|