Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.46 g/cm³ Show Material materials with Dichte of 1.46 g/cm³ | ISO 1183 |
Wasserabsorption | 23.0 °C | 0.4 % Show Material materials with Wasserabsorption of 0.4 % | Sim. to ISO 62 | Immersion 24h |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegemodul | 23.0 °C | 10.3 GPa Show Material materials with Biegemodul of 10.3 GPa | ISO 178 |
Dehnung | 23.0 °C | 2.3 % Show Material materials with Dehnung of 2.3 % | ISO 527-1/-2 |
Elastizitätsmodul | 23.0 °C | 12 GPa Show Material materials with Elastizitätsmodul of 12 GPa | ISO 527-1/-2 |
Poissonzahl | 23.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | |
Schlagfestigkeit, Charpy gekerbt | -6.0 °C | 7 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 7 kJ/m² | ISO 179/1eA |
23.0 °C | 9 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 9 kJ/m² | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -6.0 °C | 40 kJ/m² Show Material materials with Schlagzähigkeit, Charpy ungekerbt of 40 kJ/m² | ISO 179/1eU |
23.0 °C | 45 kJ/m² Show Material materials with Schlagzähigkeit, Charpy ungekerbt of 45 kJ/m² | ISO 179/1eU | |
Zugfestigkeit | 23.0 °C | 200 MPa Show Material materials with Zugfestigkeit of 200 MPa | ISO 527-1/-2 |
Thermisch
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Glasübergangstemperatur | 90 °C Show Material materials with Glasübergangstemperatur of 90 °C | ISO 11357-1/-2 | 18°F/min | |||
Heat deflection temperature, 1.80 MPa | 285 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 285 °C | ISO 75-1/-2 | |||
Koeffizient der thermischen Ausdehnung | 23.0 °C | 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1E-5 1/K | ISO 11359-1/-2 | -40 - 23°C | ||
Relative temperature index, electrical | 150 °C Show Material materials with Relative temperature index, electrical of 150 °C | UL 746B | 120mil | |||
Relative temperature index, mechanical impact | 125 °C Show Material materials with Relative temperature index, mechanical impact of 125 °C | UL 746B | 120mil | |||
Relative temperature index, mechanical strength | 150 °C Show Material materials with Relative temperature index, mechanical strength of 150 °C | UL 746B | 120mil | |||
Schmelzpunkt | 310 °C Show Material materials with Schmelzpunkt of 310 °C | ISO 11357-1/-3 | first heat | |||
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 8E-5 1/K Show Material materials with thermischer Ausdehnungskoeffizient, transversal of 8E-5 1/K | ISO 11359-1/-2 | 55 - 160°C | ||
Entflammbarkeit | Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: HB class, Thickness tested: 0.75 mm, UL recognition: yes -, Glow Wire Flammability Index, 30mil: 750 °C, Glow Wire Flammability Index, 60mil: 700 °C, Glow Wire Flammability Index, 120mil: 850 °C, Glow Wire Ignition Temperature, 30mil: 775 °C, Glow Wire Ignition Temperature, 60mil: 725 °C, Glow Wire Ignition Temperature, 120mil: 775 °C, FMVSS Class: B -, Burning rate, Thickness 1 mm: 44 mm/min |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Durchschlagfestigkeit | 23.0 °C | 34 kV/mm Show Material materials with Durchschlagfestigkeit of 34 kV/mm | IEC 60243-1 |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Material materials with Volume resistivity of 1.00E+15 Ω·cm | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Fillers | 35% Glass Fiber | |
Processing methods | Drying Recommended: yes, Drying Temperature: 100°C, Drying Time, Dehumidified Dryer: 6-8h, Processing Moisture Content: ≤0.1%, Melt Temperature Optimum: 325°C, Min. melt temperature: 320°C, Max. melt temperature: 330°C, Min. mold temperature: 90°C, Max. mold temperature: 110°C |