Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 1.05 g/cm³ Show Material materials with Dichte of 1.05 g/cm³ |
Relative Dichte | 23.0 °C | 1.05 [-] Show Material materials with Relative Dichte of 1.05 [-] |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegemodul | -40.0 °C | 2.28 GPa Show Material materials with Biegemodul of 2.28 GPa | |
23.0 °C | 0.31 GPa Show Material materials with Biegemodul of 0.31 GPa | ||
80.0 °C | 0.16 GPa Show Material materials with Biegemodul of 0.16 GPa | ||
Dehnung | -40.0 °C | 220 % Show Material materials with Dehnung of 220 % | |
23.0 °C | 380 % Show Material materials with Dehnung of 380 % | ||
80.0 °C | 420 % Show Material materials with Dehnung of 420 % | ||
Elongation at yield | 23.0 °C | 26 % Show Material materials with Elongation at yield of 26 % | |
Hardness, Rockwell R | 23.0 °C | 75 [-] Show Material materials with Hardness, Rockwell R of 75 [-] | |
Härte, Shore D | 23.0 °C | 63 [-] Show Material materials with Härte, Shore D of 63 [-] | |
Schlagzähigkeit, Izod ungekerbt | -40.0 °C | 21 kJ/m² Show Material materials with Schlagzähigkeit, Izod ungekerbt of 21 kJ/m² | No Break @ 23,80°C |
Streckgrenze | 23.0 °C | 21 MPa Show Material materials with Streckgrenze of 21 MPa | |
Zugfestigkeit | -40.0 °C | 76 MPa Show Material materials with Zugfestigkeit of 76 MPa | |
23.0 °C | 62 MPa Show Material materials with Zugfestigkeit of 62 MPa | ||
80.0 °C | 54 MPa Show Material materials with Zugfestigkeit of 54 MPa | ||
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Glasübergangstemperatur | 41.85 °C Show Material materials with Glasübergangstemperatur of 41.85 °C | ||
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.1E-4 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-4 1/K | for -30 to 50°C |
Schmelzpunkt | 183.85 °C Show Material materials with Schmelzpunkt of 183.85 °C | ||
Schmelzwärme | 39 J/g Show Material materials with Schmelzwärme of 39 J/g | 24% crystallinity | |
Wärmeformbeständigkeitstemperatur | 39.85 °C Show Material materials with Wärmeformbeständigkeitstemperatur of 39.85 °C | ||
Wärmeleitfähigkeit | 23.0 °C | 0.19 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 0.19 W/(m·K) |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dielektrizitätskonstante, 1 MHz | 23.0 °C | 3.1 [-] Show Material materials with Dielektrizitätskonstante, 1 MHz of 3.1 [-] | Dry |
Dissipation factor, 1MHz | 23.0 °C | 0.04 [-] Show Material materials with Dissipation factor, 1MHz of 0.04 [-] | Dry |
Durchschlagfestigkeit | 23.0 °C | 24 kV/mm Show Material materials with Durchschlagfestigkeit of 24 kV/mm |
Technological properties
Property | ||
---|---|---|
Application areas | Tubing, hoses, and pipes for automotive, trucking, industrial, and petroleum production applications. Examples are heavy truck airbrake tubing, automotive fuel lines, and submarine flexible pipes for offshore oil production. Thermoplastic powder coatings for industrial, transportation, and retail items are prepared in a Nylon 11 base. Nylon 11 is being used in a variety of food-contact applications, including sausage casing, beverage tubing, and reusable kitchen devices. |