Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 7.5 g/cm³ Show Material materials with Dichte of 7.5 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Charpy impact energy, V-notch | 23.0 °C | 27 J Show Material materials with Charpy impact energy, V-notch of 27 J |
Dehnung | 23.0 °C | 17 % Show Material materials with Dehnung of 17 % |
Streckgrenze Rp 0,2 | 23.0 °C | 245 - 325 MPa Show Material materials with Streckgrenze Rp 0,2 of 245 - 325 MPa |
Zugfestigkeit | 23.0 °C | 620 - 680 MPa Show Material materials with Zugfestigkeit of 620 - 680 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | for 0-300°C |
Schmelzpunkt | 1060 - 1075 °C Show Material materials with Schmelzpunkt of 1060 - 1075 °C | ||
Wärmeleitfähigkeit | 23.0 °C | 59 - 67 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 59 - 67 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 23.0 °C | 6.96E+6 - 8.12E+6 S/m Show Material materials with Elektrische Leitfähigkeit of 6.96E+6 - 8.12E+6 S/m |
Specific Electrical conductivity | 12 - 14 % IACS Show Material materials with Specific Electrical conductivity of 12 - 14 % IACS |
Magnetisch
Property | Temperature | Value |
---|---|---|
Relative magnetische Permeabilität | 23.0 °C | 1.5 [-] Show Material materials with Relative magnetische Permeabilität of 1.5 [-] |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminium | 8.5 - 10 % Show Material materials with Aluminium of 8.5 - 10 % | ||
Eisen | 4 - 5 % Show Material materials with Eisen of 4 - 5 % | ||
Kupfer | Balance | ||
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | max. | |
Nickel | 4.5 - 5.5 % Show Material materials with Nickel of 4.5 - 5.5 % |
Technological properties
Property | ||
---|---|---|
Application areas | Offshore & marine: High performance fasteners, valve and pump components, propeller shafts and weapons handling systems;Other: Pipe fittings, heat exchangers, wear plates, thrust washers, bearings, bushes, safety tools, worm wheels and gears | |
Corrosion properties | Excellent resistance to erosion and corrosion |