Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 7.6 g/cm³ Show Material materials with Dichte of 7.6 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 23.0 °C | 5 - 12 % Show Material materials with Dehnung of 5 - 12 % |
Streckgrenze Rp 0,2 | 23.0 °C | 275 - 415 MPa Show Material materials with Streckgrenze Rp 0,2 of 275 - 415 MPa |
Zugfestigkeit | 23.0 °C | 550 - 760 MPa Show Material materials with Zugfestigkeit of 550 - 760 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | for 0-300°C |
Schmelzpunkt | 1050 - 1070 °C Show Material materials with Schmelzpunkt of 1050 - 1070 °C | ||
Wärmeleitfähigkeit | 23.0 °C | 38 - 46 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 - 46 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 23.0 °C | 4.06E+6 - 5.22E+6 S/m Show Material materials with Elektrische Leitfähigkeit of 4.06E+6 - 5.22E+6 S/m |
Specific Electrical conductivity | 7 - 9 % IACS Show Material materials with Specific Electrical conductivity of 7 - 9 % IACS |
Magnetisch
Property | Temperature | Value |
---|---|---|
Relative magnetische Permeabilität | 23.0 °C | 1 [-] Show Material materials with Relative magnetische Permeabilität of 1 [-] |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminium | 9 - 11 % Show Material materials with Aluminium of 9 - 11 % | ||
Eisen | 2 - 4 % Show Material materials with Eisen of 2 - 4 % | ||
Kupfer | Balance | ||
Mangan | 1.5 % Show Material materials with Mangan of 1.5 % | max. | |
Nickel | 4 - 5.5 % Show Material materials with Nickel of 4 - 5.5 % | ||
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % |
Technological properties
Property | ||
---|---|---|
Application areas | Offshore & marine: Marine fasteners, hardware and fittings;Aerospace: Landing gear components, thrust washers, gears, control bushes, faucet balls, springs and worm wheels;Other: Non-sparking safety tooling, valve stems and seats, wear plates, welding clamps, valve spindles and components, fasteners and bearing bushes | |
Corrosion properties | High resistance to corrosion and erosion | |
General machinability | Good machinability | |
Hot forming | Easily hot worked |