Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Charpy impact energy, V-notch | 23.0 °C | 33 J Show Material materials with Charpy impact energy, V-notch of 33 J |
Dehnung | 23.0 °C | 9 - 20 % Show Material materials with Dehnung of 9 - 20 % |
Streckgrenze Rp 0,2 | 23.0 °C | 220 - 310 MPa Show Material materials with Streckgrenze Rp 0,2 of 220 - 310 MPa |
Zugfestigkeit | 23.0 °C | 515 - 620 MPa Show Material materials with Zugfestigkeit of 515 - 620 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | for 0-300°C |
Schmelzpunkt | 980 - 1010 °C Show Material materials with Schmelzpunkt of 980 - 1010 °C | ||
Wärmeleitfähigkeit | 23.0 °C | 45 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 23.0 °C | 4.06E+6 - 5.22E+6 S/m Show Material materials with Elektrische Leitfähigkeit of 4.06E+6 - 5.22E+6 S/m |
Specific Electrical conductivity | 7 - 8 % IACS Show Material materials with Specific Electrical conductivity of 7 - 8 % IACS |
Magnetisch
Property | Temperature | Value |
---|---|---|
Relative magnetische Permeabilität | 23.0 °C | 1 [-] Show Material materials with Relative magnetische Permeabilität of 1 [-] |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminium | 6 - 6.4 % Show Material materials with Aluminium of 6 - 6.4 % | ||
Eisen | 0.5 - 0.7 % Show Material materials with Eisen of 0.5 - 0.7 % | ||
Kupfer | Balance | ||
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | max. | |
Silizium | 2 - 2.4 % Show Material materials with Silizium of 2 - 2.4 % |
Technological properties
Property | ||
---|---|---|
Application areas | Offshore & marine: High strength and non-magnetic fasteners and components;Other: Fasteners, safety tooling, valve components, non-magnetic parts, marine hardware, gears, bearings and bushes and instrumentation components | |
Corrosion properties | Excellent corrosion resistance | |
General machinability | Good machinability |