Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.53 g/cm³ Show Material materials with Dichte of 8.53 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 23.0 °C | 20 % Show Material materials with Dehnung of 20 % |
Elastizitätsmodul | 23.0 °C | 105 GPa Show Material materials with Elastizitätsmodul of 105 GPa |
Härte, Brinell | 23.0 °C | 75 - 95 [-] Show Material materials with Härte, Brinell of 75 - 95 [-] |
Streckgrenze Rp 0,2 | 23.0 °C | 260 MPa Show Material materials with Streckgrenze Rp 0,2 of 260 MPa |
Zugfestigkeit | 23.0 °C | 485 MPa Show Material materials with Zugfestigkeit of 485 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Schmelzpunkt | 970 - 1025 °C Show Material materials with Schmelzpunkt of 970 - 1025 °C | |
Wärmeleitfähigkeit | 23.0 °C | 36 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 W/(m·K) |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Eisen | 0.8 % Show Material materials with Eisen of 0.8 % | max. | |
Kupfer | Balance | ||
Mangan | 0.5 - 1.3 % Show Material materials with Mangan of 0.5 - 1.3 % | ||
Silizium | 2.8 - 3.8 % Show Material materials with Silizium of 2.8 - 3.8 % | ||
Zink | 1.5 % Show Material materials with Zink of 1.5 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | Architectural & decorative: Furniture, fire place surrounds, nameplates, sculptures, signs, bolts, cladding, door and window frames, hinge pins, latches, masonry fixings, slate and tile nails, panels, spring brackets, screws, step irons, tension bolts and wall ties;Electrical: current-carrying electrical components such as slip rings, squirrel cages, springs, rotary switch contacts, contact blades, short-circuit rings, heavy-duty switchgear, bearing plates, bolts, busbar clamps, bushes, clutch discs, cotter pins, electrical conduit, fasteners, locking washers, piston rings, thrust washers and u-bolts;Automotive: valve guides, bushes and valve seats;Chemical processing: Autoclaves, chemical apparatus, drains, explosives plant, fans and ducts for corrosive vapours, fasteners, heat exchanger tube plates, filters, pickling and recovery plant, pressure vessels, pump rods and shafts, screen plates, stirrers, valve stems, vats and washers;Offshore & marine: Fasteners, propeller shafts, hull and deck fittings, fuel and water tanks, non-magnetic instrumentation, subsea electromechanical equipment and other hardware | |
Cold Forming | Excellent cold formability | |
Corrosion properties | Excellent corrosion resistance | |
Hot forming | Excellent hort formability, Hot Working Temperature (°C): 710-870 |