Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.44 g/cm³ Show Material materials with Dichte of 8.44 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 23.0 °C | 14 - 20 % Show Material materials with Dehnung of 14 - 20 % |
Elastizitätsmodul | 23.0 °C | 179 GPa Show Material materials with Elastizitätsmodul of 179 GPa |
Härte, Rockwell C | 23.0 °C | 27 - 35 [-] Show Material materials with Härte, Rockwell C of 27 - 35 [-] |
Streckgrenze Rp 0,2 | 23.0 °C | 690 - 760 MPa Show Material materials with Streckgrenze Rp 0,2 of 690 - 760 MPa |
Zugfestigkeit | 23.0 °C | 970 - 1000 MPa Show Material materials with Zugfestigkeit of 970 - 1000 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.34E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.34E-5 1/K |
Schmelzpunkt | 1315 - 1350 °C Show Material materials with Schmelzpunkt of 1315 - 1350 °C | |
Wärmeleitfähigkeit | 23.0 °C | 17.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 17.5 W/(m·K) |
Elektrisch
Property | Value |
---|---|
Specific Electrical conductivity | 28 % IACS Show Material materials with Specific Electrical conductivity of 28 % IACS |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 2.3 - 3.15 % Show Material materials with Aluminium of 2.3 - 3.15 % | |
Eisen | 2 % Show Material materials with Eisen of 2 % | max. |
Kupfer | 27 - 33 % Show Material materials with Kupfer of 27 - 33 % | |
Nickel | 63 % Show Material materials with Nickel of 63 % | min., (Ni+Co) |
Titan | 0.35 - 0.85 % Show Material materials with Titan of 0.35 - 0.85 % |
Technological properties
Property | ||
---|---|---|
Application areas | Offshore & marine: Marine propeller shafts, pump shafts, impellers, valve trim, drill collars, high strength fasteners and bolting;Other: Oil well surveying equipment, cryogenic equipment springs and electronic components | |
Cold Forming | It can be cold worked | |
Corrosion properties | Excellent corrosion resistance in marine environments | |
General machinability | It is readily machinable | |
Hot forming | It can be hot worked |