Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.12 g/cm³ Show Material materials with Dichte of 8.12 g/cm³ |
Abmessung
Property | Value |
---|---|
Breite | 381 mm Show Material materials with Breite of 381 mm |
Dicke | 4.8 - 7.1 mm Show Material materials with Dicke of 4.8 - 7.1 mm |
Länge | 1828 mm Show Material materials with Länge of 1828 mm |
Dimensions | Available thicknesses: 4.8mm, 7.1mm |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 23.0 °C | 30 % Show Material materials with Dehnung of 30 % | in 2 in. |
Elastizitätsmodul | 23.0 °C | 148 GPa Show Material materials with Elastizitätsmodul of 148 GPa | |
Härte, Rockwell B | 23.0 °C | 80 [-] Show Material materials with Härte, Rockwell B of 80 [-] | |
Streckgrenze | 23.0 °C | 235 MPa Show Material materials with Streckgrenze of 235 MPa | |
Zugfestigkeit | 23.0 °C | 566 MPa Show Material materials with Zugfestigkeit of 566 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 4.2E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 4.2E-6 1/K | from 30°C to the mentioned temperature |
150.0 °C | 4.2E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
200.0 °C | 4.2E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
250.0 °C | 4.2E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
300.0 °C | 4E-6 - 4.7E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 4E-6 - 4.7E-6 1/K | from 30°C to the mentioned temperature | |
325.0 °C | 4.6E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 4.6E-6 1/K | from 30°C to the mentioned temperature | |
350.0 °C | 5E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 5E-6 1/K | from 30°C to the mentioned temperature | |
375.0 °C | 5.6E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 5.6E-6 1/K | from 30°C to the mentioned temperature | |
400.0 °C | 6.1E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 6.1E-6 1/K | from 30°C to the mentioned temperature | |
425.0 °C | 6.7E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 6.7E-6 1/K | from 30°C to the mentioned temperature | |
450.0 °C | 6.7E-6 - 7.4E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 6.7E-6 - 7.4E-6 1/K | from 30°C to the mentioned temperature | |
475.0 °C | 7.7E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.7E-6 1/K | from 30°C to the mentioned temperature | |
500.0 °C | 8.1E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.1E-6 1/K | from 30°C to the mentioned temperature | |
525.0 °C | 8.5E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.5E-6 1/K | from 30°C to the mentioned temperature | |
550.0 °C | 8.9E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.9E-6 1/K | from 30°C to the mentioned temperature | |
600.0 °C | 9.6E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.6E-6 1/K | from 30°C to the mentioned temperature | |
700.0 °C | 1.05E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 1/K | from 30°C to the mentioned temperature | |
800.0 °C | 1.14E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.14E-5 1/K | from 30°C to the mentioned temperature | |
900.0 °C | 1.23E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.23E-5 1/K | from 30°C to the mentioned temperature | |
1004.0 °C | 1.32E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32E-5 1/K | from 30°C to the mentioned temperature | |
Schmelzpunkt | 1427 °C Show Material materials with Schmelzpunkt of 1427 °C | ||
Spezifische Wärmekapazität | 23.0 °C | 502 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 502 J/(kg·K) | |
Wärmeleitfähigkeit | 23.0 °C | 11 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 11 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 23.0 °C | 6.8E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.8E-7 Ω·m |
Magnetisch
Property | Value |
---|---|
Curie-Temperatur | 380 °C Show Material materials with Curie-Temperatur of 380 °C |
Chemical properties
Property | Value |
---|---|
Chrom | 0.03 % Show Material materials with Chrom of 0.03 % |
Eisen | Balance |
Kohlenstoff | 0.05 % Show Material materials with Kohlenstoff of 0.05 % |
Nickel | 41 % Show Material materials with Nickel of 41 % |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % |
Technological properties
Property | ||
---|---|---|
Application areas | Common applications of Alloy 42: Thermostats, thermoswitches, integrated circuit lead frames, Glass to metal seals for a wide variety of electronic tubes, hermetic packages, and automotive and industrial lamps., high temperature curing of aircraft thermoset composites |