Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.17 g/cm³ Show Material materials with Dichte of 8.17 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 23.0 °C | 30 % Show Material materials with Dehnung of 30 % | in 2 in. |
Elastizitätsmodul | 23.0 °C | 159 GPa Show Material materials with Elastizitätsmodul of 159 GPa | |
Härte, Rockwell B | 23.0 °C | 80 [-] Show Material materials with Härte, Rockwell B of 80 [-] | |
Streckgrenze | 23.0 °C | 242 MPa Show Material materials with Streckgrenze of 242 MPa | |
Zugfestigkeit | 23.0 °C | 552 MPa Show Material materials with Zugfestigkeit of 552 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 8.2E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.2E-6 1/K | from 30°C to the mentioned temperature |
150.0 °C | 8.1E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.1E-6 1/K | from 30°C to the mentioned temperature | |
200.0 °C | 7.9E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.9E-6 1/K | from 30°C to the mentioned temperature | |
250.0 °C | 7.8E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.8E-6 1/K | from 30°C to the mentioned temperature | |
300.0 °C | 7.5E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.5E-6 1/K | from 30°C to the mentioned temperature | |
350.0 °C | 7.1E-6 - 7.8E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.1E-6 - 7.8E-6 1/K | from 30°C to the mentioned temperature | |
375.0 °C | 7.5E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.5E-6 1/K | from 30°C to the mentioned temperature | |
400.0 °C | 7.5E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.5E-6 1/K | from 30°C to the mentioned temperature | |
425.0 °C | 7.6E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.6E-6 1/K | from 30°C to the mentioned temperature | |
450.0 °C | 7.9E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.9E-6 1/K | from 30°C to the mentioned temperature | |
500.0 °C | 8.2E-6 - 8.9E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.2E-6 - 8.9E-6 1/K | from 30°C to the mentioned temperature | |
550.0 °C | 9.3E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.3E-6 1/K | from 30°C to the mentioned temperature | |
600.0 °C | 9.8E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.8E-6 1/K | from 30°C to the mentioned temperature | |
700.0 °C | 1.07E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.07E-5 1/K | from 30°C to the mentioned temperature | |
800.0 °C | 1.16E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.16E-5 1/K | from 30°C to the mentioned temperature | |
900.0 °C | 1.25E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25E-5 1/K | from 30°C to the mentioned temperature | |
1000.0 °C | 1.34E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.34E-5 1/K | from 30°C to the mentioned temperature | |
Schmelzpunkt | 1427 °C Show Material materials with Schmelzpunkt of 1427 °C | ||
Spezifische Wärmekapazität | 23.0 °C | 502 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 502 J/(kg·K) | |
Wärmeleitfähigkeit | 23.0 °C | 11 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 11 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 23.0 °C | 4.7E-7 Ω·m Show Material materials with spezifischer Widerstand of 4.7E-7 Ω·m |
Magnetisch
Property | Value |
---|---|
Curie-Temperatur | 460 °C Show Material materials with Curie-Temperatur of 460 °C |
Chemical properties
Property | Value |
---|---|
Chrom | 0.03 % Show Material materials with Chrom of 0.03 % |
Eisen | Balance |
Kohlenstoff | 0.05 % Show Material materials with Kohlenstoff of 0.05 % |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % |
Nickel | 46 % Show Material materials with Nickel of 46 % |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % |
Technological properties
Property | ||
---|---|---|
Application areas | Common applications of Alloy 42: Thermostats, thermoswitches, integrated circuit lead frames, select glass-to-metal sealing applications, high temperature curing of aircraft thermoset composites |