Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.3 g/cm³ Show Material materials with Dichte of 8.3 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 23.0 °C | 35 % Show Material materials with Dehnung of 35 % | in 2 in. |
Elastizitätsmodul | 23.0 °C | 159 GPa Show Material materials with Elastizitätsmodul of 159 GPa | |
Härte, Rockwell B | 23.0 °C | 80 [-] Show Material materials with Härte, Rockwell B of 80 [-] | |
Streckgrenze | 23.0 °C | 276 MPa Show Material materials with Streckgrenze of 276 MPa | |
Zugfestigkeit | 23.0 °C | 552 MPa Show Material materials with Zugfestigkeit of 552 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.05E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 1/K | from 30°C to the mentioned temperature |
150.0 °C | 1.05E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 1/K | from 30°C to the mentioned temperature | |
200.0 °C | 1.04E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
250.0 °C | 1.04E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
300.0 °C | 1.02E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.02E-5 1/K | from 30°C to the mentioned temperature | |
350.0 °C | 1.02E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.02E-5 1/K | from 30°C to the mentioned temperature | |
400.0 °C | 1.01E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.01E-5 1/K | from 30°C to the mentioned temperature | |
450.0 °C | 1.07E-5 - 9.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.07E-5 - 9.6E-5 1/K | from 30°C to the mentioned temperature | |
475.0 °C | 1.01E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.01E-5 1/K | from 30°C to the mentioned temperature | |
500.0 °C | 1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-5 1/K | from 30°C to the mentioned temperature | |
525.0 °C | 1.04E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
550.0 °C | 1.02E-5 - 1.07E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.02E-5 - 1.07E-5 1/K | from 30°C to the mentioned temperature | |
600.0 °C | 1.08E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08E-5 1/K | from 30°C to the mentioned temperature | |
700.0 °C | 1.17E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.17E-5 1/K | from 30°C to the mentioned temperature | |
800.0 °C | 1.25E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25E-5 1/K | from 30°C to the mentioned temperature | |
900.0 °C | 1.33E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.33E-5 1/K | from 30°C to the mentioned temperature | |
1009.0 °C | 1.42E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.42E-5 1/K | from 30°C to the mentioned temperature | |
Schmelzpunkt | 1427 °C Show Material materials with Schmelzpunkt of 1427 °C | ||
Spezifische Wärmekapazität | 23.0 °C | 502 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 502 J/(kg·K) | |
Wärmeleitfähigkeit | 23.0 °C | 14 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 14 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 23.0 °C | 4.4E-7 Ω·m Show Material materials with spezifischer Widerstand of 4.4E-7 Ω·m |
Magnetisch
Property | Value |
---|---|
Curie-Temperatur | 530 °C Show Material materials with Curie-Temperatur of 530 °C |
Chemical properties
Property | Value |
---|---|
Chrom | 0.03 % Show Material materials with Chrom of 0.03 % |
Eisen | Balance |
Kohlenstoff | 0.05 % Show Material materials with Kohlenstoff of 0.05 % |
Nickel | 50.5 % Show Material materials with Nickel of 50.5 % |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % |
Technological properties
Property | ||
---|---|---|
Application areas | Common applications of Alloy 52: Pin feed-throughs for semiconductor devices, glass-to-metal sealing with soft glass for mercury switches and semiconductor devices |