Structural Epoxy Resin T26 (EP-CF)

Want to keep this datasheet? Save it now in your required format

Description

Т26 is a single part low viscosity epoxy infusion carbon fiber reinforced resin developed for high-loaded structures. T26 offers simple and flexible processing due to low viscosity at relatively low impregnation temperatures (110°С). T26 was developed specially for RTM and vacuum infusion molding, to produce laminates with low porosity and extremely high mechanical performance, especially in crack resistance. It shows the following features and properties:


  • One-part resin designed specifically for high-temperature infusion or RTM
  • Wide processing window > 7 hours at 110°C
  • Curing at 180°C provides glass transition temperature of 205°C
  • High wet glass transition temperature —172°C
  • Very high resistance to impact
  • Operating temperatures from –60°C to 150°C
  • Diese Materialdaten wurden von Matmatch zur Verfügung gestellt

    Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
    Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

    Ashby charts

    Eigenschaften

    Mechanisch

    PropertyTemperatureValueComment

    Druckfestigkeit

    23.0 °C

    643 MPa

    Show Material materials with Druckfestigkeit of 643 MPa

    ASTM D6641

    Druckfestigkeit, transversal

    23.0 °C

    679 MPa

    Show Material materials with Druckfestigkeit, transversal of 679 MPa

    ASTM D6641

    Elastizitätsmodul

    23.0 °C

    65 GPa

    Show Material materials with Elastizitätsmodul of 65 GPa

    ASTM D3039

    Elastizitätsmodul, transversal

    23.0 °C

    66 GPa

    Show Material materials with Elastizitätsmodul, transversal of 66 GPa

    ASTM D3039

    Shear modulus, G₁₂

    23.0 °C

    4.5 GPa

    Show Material materials with Shear modulus, G₁₂ of 4.5 GPa

    ASTM D5379

    Shear strength, τ₁₂

    23.0 °C

    84 MPa

    Show Material materials with Shear strength, τ₁₂ of 84 MPa

    Shear strength, τ₁₃

    25.0 °C

    74 MPa

    Show Material materials with Shear strength, τ₁₃ of 74 MPa

    ASTM D2344

    120.0 °C

    51 MPa

    Show Material materials with Shear strength, τ₁₃ of 51 MPa

    ASTM D2344

    150.0 °C

    45 MPa

    Show Material materials with Shear strength, τ₁₃ of 45 MPa

    ASTM D2344

    Zugfestigkeit

    23.0 °C

    910 MPa

    Show Material materials with Zugfestigkeit of 910 MPa

    ASTM D3039

    Zugfestigkeit, transversal

    23.0 °C

    881 MPa

    Show Material materials with Zugfestigkeit, transversal of 881 MPa

    ASTM D3039

    Formänderungsenergieabgabe

    ASTM D5528

    Technological properties

    Property
    Application areas

    Drones;Sports equipment: Frame, wheels, seat, seat post, handlebar, head stem and crank arm of a sports bicycle are made of carbon composite;Geometry strengthen elements: Experimental stringer panel

    Processing history

    Samples for testing were obtained by vacuum infusion based on T26 resin and carbon fabric (CF) 22508 (sateen 8H, 200 g/m2, 3K, 3.95 GPa).

    Processing methods

    Preheat the resin to 60-90°С in its container for transfer to the resin pot. Degas the resin for 30-40 minutes while heating to 90°С. Preheat the tool to 100-110°С (or to 115-120°С for parts having complex shape or for UD parts). Maintaining resin pot temperature of 95 °С and tool temperature of 100-115 °С, begin resin infusion. After complete impregnation increase tool temperature at 2°С/min to 180°С. Dwell at 180°С for 3 h. Cool the tool to 90°С at <5°С/min before releasing part from tool.