Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 20.0 °C | 0.91 g/cm³ Show Material materials with Dichte of 0.91 g/cm³ | |
Filmstärke | 20.0 °C | 27.47 - 54.95 m²/kg Show Material materials with Filmstärke of 27.47 - 54.95 m²/kg | |
Oberflächendichte | 20.0 °C | 1.82E-3 - 3.64E-3 g/cm² Show Material materials with Oberflächendichte of 1.82E-3 - 3.64E-3 g/cm² | |
Schrumpfung | 120.0 °C | 4 - 5 % Show Material materials with Schrumpfung of 4 - 5 % | GOST 18616, ISO 11501, ASTM D1204 (Thermal shrinkage at 120˚C, 5 min) |
Schrumpfung, diagonal | 120.0 °C | 2 % Show Material materials with Schrumpfung, diagonal of 2 % | GOST 18616, ISO 11501, ASTM D1204 (Thermal shrinkage at 120˚C, 5 min) |
Abmessung
Property | Value |
---|---|
Dicke | 0.02 - 0.04 mm Show Material materials with Dicke of 0.02 - 0.04 mm |
Dimensions | Available thicknesses: 20, 25, 30, 35, 40µm. |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 200 - 220 % Show Material materials with Dehnung of 200 - 220 % | GOST 14236, ISO 527, ASTM D882 |
Dehnung, transversal | 20.0 °C | 70 - 80 % Show Material materials with Dehnung, transversal of 70 - 80 % | GOST 14236, ISO 527, ASTM D882 |
Zugfestigkeit | 20.0 °C | 130 - 140 MPa Show Material materials with Zugfestigkeit of 130 - 140 MPa | GOST 14236, ISO 527, ASTM D882 |
Zugfestigkeit, transversal | 20.0 °C | 230 - 250 MPa Show Material materials with Zugfestigkeit, transversal of 230 - 250 MPa | GOST 14236, ISO 527, ASTM D882 |
Optisch
Property | Value | Comment |
---|---|---|
Opazität | 3 - 3.2 % Show Material materials with Opazität of 3 - 3.2 % | GOST 15875, ISO 14782, ASTM D 1003 |
Technological properties
Property | ||
---|---|---|
Application areas | High quality rotogravure and flexographic solvent based printing; production of flexible packaging, requiring no fogging during packed product storage; packing lettuce, shredded vegetables, herbs, etc.; packaging for vertical VFFS and horizontal HFFS packaging machines; application temperature with packed product + 5°C; when order please specify antifog side: IN or OUT; AF side and printable side is mentioned in each roll label. | |
Friction | Kinetic coefficient of friction µ= 0.15-0.35 (GOST 27492, ISO 8295, ASTM D 1894). | |
Other | HASL BOPP films comprise: A corona treated, heat sealable skin layer with low coefficient of friction, designed for printing, a transparent, specially designed, oriented polypropylene core layer, an antifog, corona treated, heat sealable skin layer with low coefficient of friction. | |
Processing history | Treatment level: 38 mN/m (ISO 8296, ASTM D 2578) |