Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 4.506 g/cm³ Show Material materials with Dichte of 4.506 g/cm³ | Typical for Titanium |
Abmessung
Property | Temperature | Value | Shape | Comment |
---|---|---|---|---|
Dimensions | 15-65 mm diameter up to 6000 mm length °C | 7-14.5 mm diameter up to 3000 mm length | Bar | |
Durchmesser | 7 mm Show Material materials with Durchmesser of 7 mm | Bar | ||
115 mm Show Material materials with Durchmesser of 115 mm | Bar | |||
Länge | 6000 mm Show Material materials with Länge of 6000 mm | Bar | max |
Mechanisch
Property | Value | Shape | Comment |
---|---|---|---|
Dehnung | 10.0 % Show Material materials with Dehnung of 10.0 % | Bar | |
Elastizitätsmodul | 100.0 - 120.0 GPa Show Material materials with Elastizitätsmodul of 100.0 - 120.0 GPa | Typical for Titanium Alpha Alloy | |
Zugfestigkeit | 880.0 - 1080.0 MPa Show Material materials with Zugfestigkeit of 880.0 - 1080.0 MPa | Bar |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 7.599999999999997e-06 - 1.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.599999999999997e-06 - 1.1e-05 1/K | Typical for Titanium Alpha Alloy |
Schmelzpunkt | 1540.0 - 1715.0 °C Show Material materials with Schmelzpunkt of 1540.0 - 1715.0 °C | Typical for Titanium Alpha Alloy |
Spezifische Wärmekapazität | 460.0 - 527.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 460.0 - 527.0 J/(kg·K) | Typical for Titanium Alpha Alloy |
Wärmeleitfähigkeit | 4.0 - 17.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 4.0 - 17.0 W/(m·K) | Typical for Titanium Alpha Alloy |
Chemical properties
Property | Value | Shape |
---|---|---|
Aluminium | 6.2 - 7.3 % Show Material materials with Aluminium of 6.2 - 7.3 % | Bar |
Eisen | 0.2 Show Material materials with Eisen of 0.2 | Bar |
Kohlenstoff | 0.1 Show Material materials with Kohlenstoff of 0.1 | Bar |
Molybdän | 0.4 - 1.0 % Show Material materials with Molybdän of 0.4 - 1.0 % | Bar |
Niobium | 0.5 - 1.5 % Show Material materials with Niobium of 0.5 - 1.5 % | Bar |
Sauerstoff | 0.14 Show Material materials with Sauerstoff of 0.14 | Bar |
Silizium | 0.1 - 0.25 % Show Material materials with Silizium of 0.1 - 0.25 % | Bar |
Stickstoff | 0.04 Show Material materials with Stickstoff of 0.04 | Bar |
Wasserstoff | 0.015 Show Material materials with Wasserstoff of 0.015 | Bar |
Zinn | 2.0 - 3.0 % Show Material materials with Zinn of 2.0 - 3.0 % | Bar |
Zirkonium | 3.5 - 4.5 % Show Material materials with Zirkonium of 3.5 - 4.5 % | Bar |