Allgemein
Property | Value | Shape | Related Standards |
---|---|---|---|
Dichte | 4.59 g/cm³ Show Material materials with Dichte of 4.59 g/cm³ | Bar, Billet | |
4.6 g/cm³ Show Material materials with Dichte of 4.6 g/cm³ | DIN 17851 |
Abmessung
Property | Temperature | Value | Shape | Comment |
---|---|---|---|---|
Dimensions | 15-65 mm diameter up to 6000 mm length °C | 7-14.5 mm diameter up to 3000 mm length | Bar | |
Durchmesser | 7 mm Show Material materials with Durchmesser of 7 mm | Bar | ||
115 mm Show Material materials with Durchmesser of 115 mm | Bar | |||
130 mm Show Material materials with Durchmesser of 130 mm | Billet | |||
350 mm Show Material materials with Durchmesser of 350 mm | Billet | |||
Länge | 3000 mm Show Material materials with Länge of 3000 mm | Billet | ||
4500 mm Show Material materials with Länge of 4500 mm | Billet | |||
6000 mm Show Material materials with Länge of 6000 mm | Bar | max |
Mechanisch
Property | Temperature | Value | Shape | Related Standards | Comment |
---|---|---|---|---|---|
Dehnung | 12.0 % Show Material materials with Dehnung of 12.0 % | Bar, Billet | |||
Elastizitätsmodul | 114.0 GPa Show Material materials with Elastizitätsmodul of 114.0 GPa | Bar | |||
117.0 GPa Show Material materials with Elastizitätsmodul of 117.0 GPa | DIN 17851 | ||||
Flächenreduzierung | 20.0 % Show Material materials with Flächenreduzierung of 20.0 % | DIN 17851 | |||
20.0 % Show Material materials with Flächenreduzierung of 20.0 % | DIN 17851 | Transverse | |||
Härte, Brinell | 350.0 [-] Show Material materials with Härte, Brinell of 350.0 [-] | DIN 17851 | |||
Streckgrenze | 870.0 MPa Show Material materials with Streckgrenze of 870.0 MPa | DIN 17851 | RP02 | ||
920.0 MPa Show Material materials with Streckgrenze of 920.0 MPa | DIN 17851 | RP02 | |||
960.0 MPa Show Material materials with Streckgrenze of 960.0 MPa | DIN 17851 | RP02 | |||
1035.0 MPa Show Material materials with Streckgrenze of 1035.0 MPa | Bar | ||||
1050.0 MPa Show Material materials with Streckgrenze of 1050.0 MPa | DIN 17851 | RP02 | |||
Zugfestigkeit | 1000.0 MPa Show Material materials with Zugfestigkeit of 1000.0 MPa | DIN 17851 | |||
1050.0 MPa Show Material materials with Zugfestigkeit of 1050.0 MPa | DIN 17851 | ||||
1100.0 MPa Show Material materials with Zugfestigkeit of 1100.0 MPa | DIN 17851 | ||||
1138.0 MPa Show Material materials with Zugfestigkeit of 1138.0 MPa | Bar, Billet | ||||
500 °C | 750.0 MPa Show Material materials with Zugfestigkeit of 750.0 MPa | DIN 17851 |
Thermisch
Property | Temperature | Value | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 8.599999999999999e-06 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.599999999999999e-06 1/K | DIN 17851 | ||
200 °C | 8.599999999999999e-06 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.599999999999999e-06 1/K | DIN 17851 | |||
Schmelzpunkt | 1500.0 - 1750.0 °C Show Material materials with Schmelzpunkt of 1500.0 - 1750.0 °C | Typical for Titanium Alpha Beta Alloy | |||
Spezifische Wärmekapazität | 370.0 - 674.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 370.0 - 674.0 J/(kg·K) | Typical for Titanium Alpha Beta Alloy | |||
Wärmeleitfähigkeit | 7.54 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 7.54 W/(m·K) | DIN 17851 | |||
7.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 7.6 W/(m·K) | Bar |
Elektrisch
Property | Value | Related Standards |
---|---|---|
spezifischer Widerstand | 1.5e-06 Show Material materials with spezifischer Widerstand of 1.5e-06 | DIN 17851 |
Chemical properties
Property | Value | Related Standards | Shape |
---|---|---|---|
Aluminium | 3.0 - 5.0 % Show Material materials with Aluminium of 3.0 - 5.0 % | DIN 17851 | Bar, Billet |
Eisen | 0.20 % Show Material materials with Eisen of 0.20 % | DIN 17851 | |
0.2 % Show Material materials with Eisen of 0.2 % | Bar, Billet | ||
Kohlenstoff | 0.08 % Show Material materials with Kohlenstoff of 0.08 % | DIN 17851 | |
Molybdän | 3.0 - 5.0 % Show Material materials with Molybdän of 3.0 - 5.0 % | DIN 17851 | Bar, Billet |
Sauerstoff | 0.25 % Show Material materials with Sauerstoff of 0.25 % | DIN 17851 | |
0.27 % Show Material materials with Sauerstoff of 0.27 % | Bar, Billet | ||
Silizium | 0.3 - 0.7 % Show Material materials with Silizium of 0.3 - 0.7 % | DIN 17851 | Bar, Billet |
Stickstoff | 0.05 % Show Material materials with Stickstoff of 0.05 % | DIN 17851 | Bar, Billet |
Wasserstoff | 0.0125 % Show Material materials with Wasserstoff of 0.0125 % | Bar, Billet | |
0.015 % Show Material materials with Wasserstoff of 0.015 % | DIN 17851 | ||
Zinn | 1.5 - 2.5 % Show Material materials with Zinn of 1.5 - 2.5 % | DIN 17851 | Bar, Billet |