Allgemein
Property | Temperature | Value | Related Standards |
---|---|---|---|
Dichte | 20.0 °C | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | EN 573-3 |
Mechanisch
Property | Temperature | Value | Related Standards | Comment |
---|---|---|---|---|
Dehnung | -196.0 °C | 23.0 - 30.0 % Show Material materials with Dehnung of 23.0 - 30.0 % | EN 573-3 | |
-196.0 °C | 23.0 % Show Material materials with Dehnung of 23.0 % | EN 573-3 | ||
-196.0 °C | 30.0 % Show Material materials with Dehnung of 30.0 % | EN 573-3 | ||
-80.0 °C | 11.0 - 18.0 % Show Material materials with Dehnung of 11.0 - 18.0 % | EN 573-3 | ||
-80.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | EN 573-3 | ||
-80.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | EN 573-3 | ||
-28.0 °C | 10.0 - 16.0 % Show Material materials with Dehnung of 10.0 - 16.0 % | EN 573-3 | ||
-28.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | EN 573-3 | ||
-28.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | EN 573-3 | ||
20.0 °C | 10.0 - 16.0 % Show Material materials with Dehnung of 10.0 - 16.0 % | EN 573-3 | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | EN 573-3 | ||
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | EN 573-3 | ||
100.0 °C | 10.0 - 16.0 % Show Material materials with Dehnung of 10.0 - 16.0 % | EN 573-3 | ||
100.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | EN 573-3 | ||
100.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | EN 573-3 | ||
150.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | EN 573-3 | ||
150.0 °C | 11.0 - 16.0 % Show Material materials with Dehnung of 11.0 - 16.0 % | EN 573-3 | ||
150.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | EN 573-3 | ||
200.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | EN 573-3 | ||
200.0 °C | 18.0 - 20.0 % Show Material materials with Dehnung of 18.0 - 20.0 % | EN 573-3 | ||
200.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | EN 573-3 | ||
260.0 °C | 60.0 % Show Material materials with Dehnung of 60.0 % | EN 573-3 | ||
315.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | EN 573-3 | ||
370.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | EN 573-3 | ||
Elastizitätsmodul | -270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | EN 573-3 | |
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 70.0 GPa | EN 573-3 | ||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 65.0 GPa | EN 573-3 | ||
20.0 °C | 60.0 - 69.5 GPa Show Material materials with Elastizitätsmodul of 60.0 - 69.5 GPa | EN 573-3 | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 69.0 GPa | EN 573-3 | ||
20.0 °C | 65.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 65.0 - 70.0 GPa | EN 573-3 | ||
20.0 °C | 65.0 - 69.5 GPa Show Material materials with Elastizitätsmodul of 65.0 - 69.5 GPa | EN 573-3 | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 65.0 - 69.0 GPa | EN 573-3 | ||
20.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | EN 573-3 | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa | EN 573-3 | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Elastizitätsmodul of 69.0 - 69.5 GPa | EN 573-3 | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.5 - 70.0 GPa | EN 573-3 | ||
20.0 °C | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | EN 573-3 | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | EN 573-3 | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | EN 573-3 | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | EN 573-3 | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | EN 573-3 | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | EN 573-3 | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | EN 573-3 | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | EN 573-3 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | EN 573-3 | |
Schubmodule | 20.0 °C | 24.0 - 26.5 GPa Show Material materials with Schubmodule of 24.0 - 26.5 GPa | EN 573-3 | |
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Schubmodule of 24.0 - 26.1 GPa | EN 573-3 | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Schubmodule of 26.1 - 26.5 GPa | EN 573-3 | ||
20.0 °C | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | EN 573-3 | ||
Streckgrenze | -196.0 °C | 170.0 MPa Show Material materials with Streckgrenze of 170.0 MPa | EN 573-3 | RP02 |
-196.0 °C | 170.0 - 230.0 MPa Show Material materials with Streckgrenze of 170.0 - 230.0 MPa | EN 573-3 | RP02 | |
-196.0 °C | 230.0 MPa Show Material materials with Streckgrenze of 230.0 MPa | EN 573-3 | RP02 | |
-80.0 °C | 150.0 MPa Show Material materials with Streckgrenze of 150.0 MPa | EN 573-3 | RP02 | |
-80.0 °C | 150.0 - 200.0 MPa Show Material materials with Streckgrenze of 150.0 - 200.0 MPa | EN 573-3 | RP02 | |
-80.0 °C | 200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | EN 573-3 | RP02 | |
-28.0 °C | 140.0 MPa Show Material materials with Streckgrenze of 140.0 MPa | EN 573-3 | RP02 | |
-28.0 °C | 140.0 - 190.0 MPa Show Material materials with Streckgrenze of 140.0 - 190.0 MPa | EN 573-3 | RP02 | |
-28.0 °C | 190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | EN 573-3 | RP02 | |
57.0 MPa Show Material materials with Streckgrenze of 57.0 MPa | ||||
20.0 °C | 140.0 MPa Show Material materials with Streckgrenze of 140.0 MPa | EN 573-3 | RP02 | |
20.0 °C | 140.0 - 185.0 MPa Show Material materials with Streckgrenze of 140.0 - 185.0 MPa | EN 573-3 | RP02 | |
20.0 °C | 185.0 MPa Show Material materials with Streckgrenze of 185.0 MPa | EN 573-3 | RP02 | |
100.0 °C | 130.0 MPa Show Material materials with Streckgrenze of 130.0 MPa | EN 573-3 | RP02 | |
100.0 °C | 130.0 - 145.0 MPa Show Material materials with Streckgrenze of 130.0 - 145.0 MPa | EN 573-3 | RP02 | |
100.0 °C | 145.0 MPa Show Material materials with Streckgrenze of 145.0 MPa | EN 573-3 | RP02 | |
150.0 °C | 110.0 MPa Show Material materials with Streckgrenze of 110.0 MPa | EN 573-3 | RP02 | |
200.0 °C | 60.0 MPa Show Material materials with Streckgrenze of 60.0 MPa | EN 573-3 | RP02 | |
260.0 °C | 30.0 MPa Show Material materials with Streckgrenze of 30.0 MPa | EN 573-3 | RP02 | |
315.0 °C | 15.0 MPa Show Material materials with Streckgrenze of 15.0 MPa | EN 573-3 | RP02 | |
370.0 °C | 10.0 MPa Show Material materials with Streckgrenze of 10.0 MPa | EN 573-3 | RP02 | |
Zugfestigkeit | -196.0 °C | 240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | EN 573-3 | |
-196.0 °C | 240.0 - 280.0 MPa Show Material materials with Zugfestigkeit of 240.0 - 280.0 MPa | EN 573-3 | ||
-196.0 °C | 280.0 MPa Show Material materials with Zugfestigkeit of 280.0 MPa | EN 573-3 | ||
-80.0 °C | 165.0 MPa Show Material materials with Zugfestigkeit of 165.0 MPa | EN 573-3 | ||
-80.0 °C | 165.0 - 220.0 MPa Show Material materials with Zugfestigkeit of 165.0 - 220.0 MPa | EN 573-3 | ||
-80.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | EN 573-3 | ||
-28.0 °C | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | EN 573-3 | ||
-28.0 °C | 150.0 - 205.0 MPa Show Material materials with Zugfestigkeit of 150.0 - 205.0 MPa | EN 573-3 | ||
-28.0 °C | 205.0 MPa Show Material materials with Zugfestigkeit of 205.0 MPa | EN 573-3 | ||
128.0 MPa Show Material materials with Zugfestigkeit of 128.0 MPa | ||||
20.0 °C | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | EN 573-3 | ||
20.0 °C | 150.0 - 200.0 MPa Show Material materials with Zugfestigkeit of 150.0 - 200.0 MPa | EN 573-3 | ||
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | EN 573-3 | ||
100.0 °C | 145.0 MPa Show Material materials with Zugfestigkeit of 145.0 MPa | EN 573-3 | ||
100.0 °C | 145.0 - 180.0 MPa Show Material materials with Zugfestigkeit of 145.0 - 180.0 MPa | EN 573-3 | ||
100.0 °C | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | EN 573-3 | ||
150.0 °C | 125.0 MPa Show Material materials with Zugfestigkeit of 125.0 MPa | EN 573-3 | ||
150.0 °C | 125.0 - 160.0 MPa Show Material materials with Zugfestigkeit of 125.0 - 160.0 MPa | EN 573-3 | ||
150.0 °C | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | EN 573-3 | ||
200.0 °C | 95.0 MPa Show Material materials with Zugfestigkeit of 95.0 MPa | EN 573-3 | ||
260.0 °C | 50.0 MPa Show Material materials with Zugfestigkeit of 50.0 MPa | EN 573-3 | ||
315.0 °C | 30.0 MPa Show Material materials with Zugfestigkeit of 30.0 MPa | EN 573-3 | ||
370.0 °C | 20.0 MPa Show Material materials with Zugfestigkeit of 20.0 MPa | EN 573-3 |
Thermisch
Property | Temperature | Value | Related Standards | Comment |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50.0 °C | 2.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.15e-05 1/K | EN 573-3 | |
2.33e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.33e-05 1/K | ||||
100.0 °C | 2.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.32e-05 1/K | EN 573-3 | ||
200.0 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | EN 573-3 | ||
300.0 °C | 2.52e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K | EN 573-3 | ||
Schmelzpunkt | 629.0 - 654.0 °C Show Material materials with Schmelzpunkt of 629.0 - 654.0 °C | Typical for Wrought 3000 Series Aluminium | ||
Spezifische Wärmekapazität | 20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 892.0 - 893.0 J/(kg·K) | EN 573-3 | |
20.0 °C | 892.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 892.0 J/(kg·K) | EN 573-3 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | EN 573-3 | ||
Wärmeleitfähigkeit | 175.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 175.0 W/(m·K) | |||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 200.0 W/(m·K) | EN 573-3 | ||
20.0 °C | 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 W/(m·K) | EN 573-3 |
Elektrisch
Property | Temperature | Value | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 22000000.0 - 29000000.0 S/m | EN 573-3 |
20.0 °C | 23000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 29000000.0 S/m | EN 573-3 | |
spezifischer Widerstand | 20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.1e-08 Ω·m | EN 573-3 |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.5e-08 Ω·m | EN 573-3 | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-08 Ω·m | EN 573-3 | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-08 - 4.5e-08 Ω·m | EN 573-3 |
Chemical properties
Property | Value | Related Standards |
---|---|---|
Eisen | 0.7 Show Material materials with Eisen of 0.7 | EN 573-3 |
Kupfer | 0.05 - 0.2 % Show Material materials with Kupfer of 0.05 - 0.2 % | EN 573-3 |
Mangan | 1.0 - 1.5 % Show Material materials with Mangan of 1.0 - 1.5 % | EN 573-3 |
Silizium | 0.6 Show Material materials with Silizium of 0.6 | EN 573-3 |
Zink | 0.1 Show Material materials with Zink of 0.1 | EN 573-3 |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |