Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.27 g/cm³ Show Material materials with Dichte of 8.27 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Flächenreduzierung | 20.0 °C | 20 % Show Material materials with Flächenreduzierung of 20 % |
650.0 °C | 12 % Show Material materials with Flächenreduzierung of 12 % | |
760.0 °C | 5 % Show Material materials with Flächenreduzierung of 5 % | |
Streckgrenze | 20.0 °C | 760 MPa Show Material materials with Streckgrenze of 760 MPa |
650.0 °C | 620 MPa Show Material materials with Streckgrenze of 620 MPa | |
760.0 °C | 480 MPa Show Material materials with Streckgrenze of 480 MPa | |
Zugfestigkeit | 20.0 °C | 1230 MPa Show Material materials with Zugfestigkeit of 1230 MPa |
650.0 °C | 940 MPa Show Material materials with Zugfestigkeit of 940 MPa | |
760.0 °C | 655 MPa Show Material materials with Zugfestigkeit of 655 MPa | |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 760.0 °C | 1.49E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49E-5 1/K | The mentioned value is between 20°C and the mentioned temperature |
Chemical properties
Property | Value |
---|---|
Aluminium | 1.4 % Show Material materials with Aluminium of 1.4 % |
Bor | 3E-3 % Show Material materials with Bor of 3E-3 % |
Chrom | 20 % Show Material materials with Chrom of 20 % |
Eisen | 55.65 - 100 % Show Material materials with Eisen of 55.65 - 100 % |
Kobalt | 18 % Show Material materials with Kobalt of 18 % |
Kohlenstoff | 0.05 % Show Material materials with Kohlenstoff of 0.05 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Silizium | 1.5 % Show Material materials with Silizium of 1.5 % |