Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.9 g/cm³ Show Material materials with Dichte of 8.9 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 18 % Show Material materials with Dehnung of 18 % | |
Elastizitätsmodul | 20.0 °C | 145 GPa Show Material materials with Elastizitätsmodul of 145 GPa | |
Härte, Brinell | 20.0 °C | 115 [-] Show Material materials with Härte, Brinell of 115 [-] | |
Poissonzahl | 23.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] | Typical for Cast Copper Nickel Grade |
Streckgrenze Rp 0,2 | 20.0 °C | 150 MPa Show Material materials with Streckgrenze Rp 0,2 of 150 MPa | |
Zugfestigkeit | 20.0 °C | 440 MPa Show Material materials with Zugfestigkeit of 440 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 300.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | |
Schmelzpunkt | 1100 - 1240 °C Show Material materials with Schmelzpunkt of 1100 - 1240 °C | Typical for Cast Copper Nickel Grade | |
Spezifische Wärmekapazität | 23.0 °C | 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 377 J/(kg·K) | Typical for Cast Copper Nickel Grade |
Wärmeleitfähigkeit | 20.0 °C | 29 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 29 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 2.50E+6 S/m Show Material materials with Elektrische Leitfähigkeit of 2.50E+6 S/m |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.01 % Show Material materials with Aluminium of 0.01 % |
Bismut | 0.01 % Show Material materials with Bismut of 0.01 % |
Blei | 0.01 % Show Material materials with Blei of 0.01 % |
Bor | 0.01 % Show Material materials with Bor of 0.01 % |
Cadmium | 0.02 % Show Material materials with Cadmium of 0.02 % |
Eisen | 0.5 - 1.5 % Show Material materials with Eisen of 0.5 - 1.5 % |
Kohlenstoff | 0.03 % Show Material materials with Kohlenstoff of 0.03 % |
Kupfer | 64 % Show Material materials with Kupfer of 64 % |
Magnesium | 0.01 % Show Material materials with Magnesium of 0.01 % |
Mangan | 0.6 - 1.2 % Show Material materials with Mangan of 0.6 - 1.2 % |
Nickel | 29 - 31 % Show Material materials with Nickel of 29 - 31 % |
Niobium | 0.5 - 1 % Show Material materials with Niobium of 0.5 - 1 % |
Phosphor | 0.01 % Show Material materials with Phosphor of 0.01 % |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % |
Selen | 0.01 % Show Material materials with Selen of 0.01 % |
Silizium | 0.3 - 0.7 % Show Material materials with Silizium of 0.3 - 0.7 % |
Tellur | 0.01 % Show Material materials with Tellur of 0.01 % |
Zink | 0.5 % Show Material materials with Zink of 0.5 % |
Technological properties
Property | ||
---|---|---|
Processing methods | sand casting, separately cast test sample |