Allgemein
Property | Temperature | Value | Related Standards |
---|---|---|---|
Dichte | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | EN 573-3 | |
20.0 °C | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | DIN 1725-1, EN 573-3, EN 573-4 |
Mechanisch
Property | Value | Comment |
---|---|---|
Elastizitätsmodul | 69.0 - 72.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 72.0 GPa | Typical for Wrought 7000 Series Aluminium |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 7000 Series Aluminium |
Schubmodule | 26.4 - 27.1 GPa Show Material materials with Schubmodule of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium |
Thermisch
Property | Temperature | Value | Related Standards | Comment |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | DIN 1725-1, EN 573-3, EN 573-4 | |
Schmelzpunkt | 465.0 - 655.0 °C Show Material materials with Schmelzpunkt of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium | ||
Spezifische Wärmekapazität | 795.0 - 1050.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium | ||
Wärmeleitfähigkeit | 20.0 °C | 122.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 122.0 W/(m·K) | DIN 1725-1, EN 573-3, EN 573-4 |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 34000000.0 S/m | Typical for Wrought 7000 Series Aluminium |
spezifischer Widerstand | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Related Standards |
---|---|---|
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | DIN 1725-1, EN 573-3, EN 573-4 |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | DIN 1725-1, EN 573-3, EN 573-4 |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | DIN 1725-1, EN 573-3, EN 573-4 |
Zink | 0.8 - 1.3 % Show Material materials with Zink of 0.8 - 1.3 % | DIN 1725-1, EN 573-3, EN 573-4 |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |