Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Dichte of 2.68 - 2.69 g/cm³ | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 8.0 % Show Material materials with Dehnung of 8.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | |
9.0 % Show Material materials with Dehnung of 9.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
13.0 % Show Material materials with Dehnung of 13.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
14.0 % Show Material materials with Dehnung of 14.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube | A50 | ||
16.0 % Show Material materials with Dehnung of 16.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | H112 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | H112 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H112 | EN 573-3 | Flat | ||
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | H112 | EN 573-3 | Sheet | ||
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H112 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H112 | EN 573-3 | Profile, Rod, Tube | ||
Elastizitätsmodul | 70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Härte, Brinell | 59.0 [-] Show Material materials with Härte, Brinell of 59.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
63.0 [-] Show Material materials with Härte, Brinell of 63.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 59.0 [-] Show Material materials with Härte, Brinell of 59.0 [-] | H112 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 59.0 - 63.0 [-] Show Material materials with Härte, Brinell of 59.0 - 63.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | H112 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 63.0 [-] Show Material materials with Härte, Brinell of 63.0 [-] | H112 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
Schubmodule | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 26.5 - 27.0 GPa Show Material materials with Schubmodule of 26.5 - 27.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Zugfestigkeit | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | H112 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | H112 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H112 | EN 573-3 | Flat | ||
20.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H112 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.1899999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1899999999999997e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
-50.0 °C | 2.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.19e-05 1/K | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20 °C | 2.1899999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1899999999999997e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
20 °C | 2.56e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.56e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
100.0 °C | 2.37e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.37e-05 1/K | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
200 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
200.0 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
300 °C | 2.56e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.56e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
300.0 °C | 2.56e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.56e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 602.0 - 646.0 °C Show Material materials with Schmelzpunkt of 602.0 - 646.0 °C | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 897.0 - 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 - 900.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 897.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Wärmeleitfähigkeit | 130.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 150.0 W/(m·K) | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 135.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 135.0 - 150.0 W/(m·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 135.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 135.0 W/(m·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 19000000.0 - 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 - 21000000.0 S/m | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 S/m | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
spezifischer Widerstand | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.76e-08 - 5.26e-08 Ω·m | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 5.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.1e-08 Ω·m | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.05 - 0.2 % Show Material materials with Chrom of 0.05 - 0.2 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
0.40 % Show Material materials with Eisen of 0.40 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Magnesium | 2.4 - 3.0 % Show Material materials with Magnesium of 2.4 - 3.0 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Mangan | 0.5 - 1.0 % Show Material materials with Mangan of 0.5 - 1.0 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |