Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
2.67 g/cm³ Show Material materials with Dichte of 2.67 g/cm³ | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | ||
20.0 °C | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | |
20.0 °C | 2.66 - 2.68 g/cm³ Show Material materials with Dichte of 2.66 - 2.68 g/cm³ | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | H111 | EN 573-3, EN 14286, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
1 °/t Show Material materials with Biegewinkel 180° of 1 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |||
2.0 °/t Show Material materials with Biegewinkel 180° of 2.0 °/t | H111 | EN 573-3, EN 14286 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
1 °/t Show Material materials with Biegewinkel 90° of 1 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
Dehnung | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | |
12 % Show Material materials with Dehnung of 12 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | A50 | ||
14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
19.0 % Show Material materials with Dehnung of 19.0 % | H111 | EN 573-3, EN 14286 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3 | Plate, Strip, Sheet, Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Tube, Rod, Plate, Strip, Sheet, Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Tube, Rod | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Plate, Strip, Sheet, Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Tube, Rod | ||
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3 | Tube, Rod, Flat | ||
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Plate, Strip, Sheet, Flat | A50 | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
Elastizitätsmodul | -270 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Strip, Plate, Rod, Flat | |
-270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Strip, Plate, Rod, Flat | ||
70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
20 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Strip, Plate, Rod, Flat | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Strip, Plate, Rod, Flat | ||
20.0 °C | 70.0 - 70.5 GPa Show Material materials with Elastizitätsmodul of 70.0 - 70.5 GPa | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
20.0 °C | 70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
300 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat | ||
Härte, Brinell | 52.0 [-] Show Material materials with Härte, Brinell of 52.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | H111 | EN 573-3 | Tube, Rod | ||
20.0 °C | 52.0 [-] Show Material materials with Härte, Brinell of 52.0 [-] | H111 | EN 573-3 | Flat | ||
Härte, HBW | 52 [-] Show Material materials with Härte, HBW of 52 [-] | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | |
Schlagfestigkeit, Charpy gekerbt | 30.0 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 30.0 kJ/m² | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
Schubmodule | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |||
20.0 °C | 26.5 - 27.0 GPa Show Material materials with Schubmodule of 26.5 - 27.0 GPa | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
20.0 °C | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
Streckgrenze | -270 °C | 80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H111 | EN 573-3 | Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar | RP02 |
-270.0 °C | 80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H111 | EN 573-3 | Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar | RP02 | |
80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | RP02 | ||
80 MPa Show Material materials with Streckgrenze of 80 MPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |||
20.0 °C | 80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H111 | EN 573-3 | Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar | RP02 | |
20 °C | 80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H111 | EN 573-3 | Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar | RP02 | |
20.0 °C | 80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H111 | EN 573-3 | Flat | RP02 Transverse | |
50.0 °C | 80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H111 | EN 573-3 | Tube, Rod, Sheet, Strip, Plate, Flat, Wire, Forging, Bar | RP02 | |
100 °C | 70.0 MPa Show Material materials with Streckgrenze of 70.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | RP02 | |
100.0 °C | 70.0 MPa Show Material materials with Streckgrenze of 70.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | RP02 | |
Zugfestigkeit | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
20.0 °C | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | H111 | EN 573-3 | Transverse | ||
20.0 °C | 180.0 - 250.0 MPa Show Material materials with Zugfestigkeit of 180.0 - 250.0 MPa | H111 | EN 573-3, EN 754, EN 755 | Tube, Rod, Strip, Sheet, Plate, Wire, Forging, Bar | ||
20.0 °C | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | H111 | EN 573-3 | Tube, Rod | ||
20.0 °C | 190.0 - 240.0 MPa Show Material materials with Zugfestigkeit of 190.0 - 240.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | H111 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 190.0 - 240.0 MPa Show Material materials with Zugfestigkeit of 190.0 - 240.0 MPa | H111 | EN 573-3, EN 14286, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Flat, Strip, Plate |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
100.0 °C | 2.39e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.39e-05 1/K | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | 20-100°C | |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 610.0 - 640.0 °C Show Material materials with Schmelzpunkt of 610.0 - 640.0 °C | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 897.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 - 963.0 J/(kg·K) | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | |
20.0 °C | 897.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 J/(kg·K) | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
20.0 °C | 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 963.0 J/(kg·K) | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
Wärmeleitfähigkeit | 147.0 - 168.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 147.0 - 168.0 W/(m·K) | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | ||
20.0 °C | 132.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 132.0 - 160.0 W/(m·K) | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
20.0 °C | 132.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 132.0 - 140.0 W/(m·K) | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
20.0 °C | 132.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 132.0 W/(m·K) | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | ||
20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K) | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 23000000.0 S/m | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Rod, Flat |
spezifischer Widerstand | 4.35e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 5e-08 Ω·m | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
4.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.9e-08 Ω·m | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | ||
20.0 °C | 4.3e-08 - 5.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.3e-08 - 5.3e-08 Ω·m | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | |
20.0 °C | 4.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.3e-08 - 5e-08 Ω·m | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | |
20.0 °C | 5e-08 - 5.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 5e-08 - 5.3e-08 Ω·m | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat | |
20.0 °C | 5.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.3e-08 Ω·m | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.1 - 0.6 % Show Material materials with Andere of 0.1 - 0.6 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar |
0.3 % Show Material materials with Chrom of 0.3 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | H111 | EN 573-3 | Tube, Plate, Strip, Sheet, Rod, Flat |
0.40 % Show Material materials with Eisen of 0.40 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
0.4 % Show Material materials with Eisen of 0.4 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar |
0.1 % Show Material materials with Kupfer of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |
Magnesium | 2.6 - 3.6 % Show Material materials with Magnesium of 2.6 - 3.6 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar, Strip, Plate |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar |
0.5 % Show Material materials with Mangan of 0.5 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar |
0.4 % Show Material materials with Silizium of 0.4 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar |
0.15 % Show Material materials with Titan of 0.15 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate | |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485, EN 754, EN 755 | Tube, Plate, Strip, Sheet, Rod, Flat, Wire, Forging, Bar |
0.2 % Show Material materials with Zink of 0.2 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Electronic devices: Housing of devices; Tubes: Industrial tubes, Pipes; Wind energy: Nacelle coverings, rotor hub, stairs; Components: Heat shields, Access hatches, Spoilers, Fuel and oil tanks, General transportation | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good to good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |