Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 13.0 % Show Material materials with Dehnung of 13.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A50 | |
15.0 % Show Material materials with Dehnung of 15.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | T4 | EN 573-3 | Profile | A50 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | T4 | EN 573-3 | Profile | ||
Elastizitätsmodul | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 73.0 GPa Show Material materials with Elastizitätsmodul of 73.0 GPa | T4 | EN 573-3 | Profile | ||
Härte, Brinell | 20.0 °C | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | T4 | EN 573-3 | Profile | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Schubmodule | 26.2 GPa Show Material materials with Schubmodule of 26.2 GPa | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | T4 | EN 573-3 | Profile | ||
Zugfestigkeit | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | T4 | EN 573-3 | Profile |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Schmelzpunkt | 585.0 - 650.0 °C Show Material materials with Schmelzpunkt of 585.0 - 650.0 °C | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Spezifische Wärmekapazität | 887.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Wärmeleitfähigkeit | 180.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 180.0 - 220.0 W/(m·K) | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 170.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 220.0 W/(m·K) | T4 | EN 573-3 | Profile |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 26000000.0 - 32000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 26000000.0 - 32000000.0 S/m | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 24000000.0 - 32000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 32000000.0 S/m | T4 | EN 573-3 | Profile | |
spezifischer Widerstand | 3.13e-08 - 3.85e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.13e-08 - 3.85e-08 Ω·m | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | T4 | EN 573-3, EN 13195, EN 755 | Profile, Strip, Sheet, Plate, Tube, Bar |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | T4 | EN 573-3 | Profile |
0.35 % Show Material materials with Eisen of 0.35 % | T4 | EN 573-3, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % | T4 | EN 573-3, EN 13195, EN 755 | Profile, Strip, Sheet, Plate, Tube, Bar |
Magnesium | 0.4 - 0.7 % Show Material materials with Magnesium of 0.4 - 0.7 % | T4 | EN 573-3, EN 13195, EN 755 | Profile, Strip, Sheet, Plate, Tube, Bar |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | T4 | EN 573-3, EN 13195, EN 755 | Profile, Strip, Sheet, Plate, Tube, Bar |
Silizium | 0.5 - 0.9 % Show Material materials with Silizium of 0.5 - 0.9 % | T4 | EN 573-3, EN 13195, EN 755 | Profile, Strip, Sheet, Plate, Tube, Bar |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | T4 | EN 573-3, EN 13195, EN 755 | Profile, Strip, Sheet, Plate, Tube, Bar |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | T4 | EN 573-3, EN 13195, EN 755 | Profile, Strip, Sheet, Plate, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / - | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable / - |