Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 8.47 g/cm³ Show Material materials with Dichte of 8.47 g/cm³ | Typical for Cast Copper Brass Yellow Brass |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A50 | 23.0 °C | 15 % Show Material materials with Dehnung A50 of 15 % | |
Elastizitätsmodul | 23.0 °C | 103 GPa Show Material materials with Elastizitätsmodul of 103 GPa | |
Härte, Rockwell B | 23.0 °C | 55 - 60 [-] Show Material materials with Härte, Rockwell B of 55 - 60 [-] | |
Kerbschlagenergie | 23.0 °C | 54 J Show Material materials with Kerbschlagenergie of 54 J | |
Poissonzahl | 23.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] | Typical for Cast Copper Brass Yellow Brass |
Streckgrenze Rp 0,2 | 23.0 °C | 207 MPa Show Material materials with Streckgrenze Rp 0,2 of 207 MPa | |
Zugfestigkeit | 23.0 °C | 379 MPa Show Material materials with Zugfestigkeit of 379 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.5E-5 - 1.9E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.5E-5 - 1.9E-5 1/K | Typical for Cast Copper Brass Yellow Brass |
Schmelzpunkt | 905 - 932 °C Show Material materials with Schmelzpunkt of 905 - 932 °C | Typical for Cast Copper Brass Yellow Brass | |
Spezifische Wärmekapazität | 23.0 °C | 335 - 390 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 335 - 390 J/(kg·K) | Typical for Cast Copper Brass Yellow Brass |
Wärmeleitfähigkeit | 23.0 °C | 116 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 116 W/(m·K) | Typical for Cast Copper Brass Yellow Brass |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.55 % Show Material materials with Aluminium of 0.55 % |
Antimon | 0.05 % Show Material materials with Antimon of 0.05 % |
Arsen | 0.05 % Show Material materials with Arsen of 0.05 % |
Blei | 1.5 % Show Material materials with Blei of 1.5 % |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % |
Kupfer | 57 % Show Material materials with Kupfer of 57 % |
Mangan | 0.25 % Show Material materials with Mangan of 0.25 % |
Nickel | 0.5 % Show Material materials with Nickel of 0.5 % |
Phosphor | 0.01 % Show Material materials with Phosphor of 0.01 % |
Schwefel | 0.05 % Show Material materials with Schwefel of 0.05 % |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % |
Zink | 31 - 41 % Show Material materials with Zink of 31 - 41 % |
Zinn | 1.5 % Show Material materials with Zinn of 1.5 % |