Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 23.0 °C | 10 - 20 % Show Material materials with Dehnung of 10 - 20 % | |
Elastizitätsmodul | 23.0 °C | 100 - 125 GPa Show Material materials with Elastizitätsmodul of 100 - 125 GPa | Typical for Wrought Copper Brass |
Härte, Rockwell B | 23.0 °C | 35 - 75 [-] Show Material materials with Härte, Rockwell B of 35 - 75 [-] | |
Schubmodule | 23.0 °C | 40 GPa Show Material materials with Schubmodule of 40 GPa | Typical for Wrought Copper Brass |
Streckgrenze Rp0,5 | 23.0 °C | 105 - 170 MPa Show Material materials with Streckgrenze Rp0,5 of 105 - 170 MPa | |
Zugfestigkeit | 23.0 °C | 275 - 450 MPa Show Material materials with Zugfestigkeit of 275 - 450 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 - 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 2.1E-5 1/K | Typical for Wrought Copper Brass |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 23.0 °C | 371 - 418 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 371 - 418 J/(kg·K) | Typical for Wrought Copper Brass |
Wärmeleitfähigkeit | 23.0 °C | 100 - 234 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 100 - 234 W/(m·K) | Typical for Wrought Copper Brass |
Chemical properties
Property | Value |
---|---|
Blei | 1.5 - 2.5 % Show Material materials with Blei of 1.5 - 2.5 % |
Eisen | 0.15 % Show Material materials with Eisen of 0.15 % |
Kupfer | 61 - 63 % Show Material materials with Kupfer of 61 - 63 % |